A foaming agent for foamed concrete based on nanoparticles and its preparation method and application
By surface hydrophobic modification of nanohydrated calcium silicate, the problem of poor stability of foam concrete is solved, the stability of foam and concrete performance are improved, and the dosage and cost of nanoparticles are reduced.
Patent Information
- Application Number
- CN202410477785.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-19
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-04-19
AI Technical Summary
During the preparation process of foam concrete, there is a problem of poor foam stability, which affects the performance of the final product, and the dosage of nanoparticles is high and the cost is high.
By performing surface hydrophobic modification on nanohydrated calcium silicate, nanohydrated calcium silicate particles with a wetting angle of 40 to 90° are obtained. During the foaming process, they are adsorbed on the air-liquid interface, reducing surface tension and improving Foam stability.
Significantly improves the stability of the foam, reduces the foam settlement and bleeding rate, enhances the compressive strength of concrete, and reduces the dosage and cost of nanoparticles.
Abstract
Description
Technical Field
[0001] The invention relates to the field of building materials, and in particular to a foam concrete foaming agent based on nanoparticles and a preparation method and application thereof. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not be necessarily regarded as an admission or any form of suggestion that the information constitutes the prior art already known to those skilled in the art.
[0003] Foamed concrete is a porous lightweight material made by preparing foam using physical and chemical methods, adding the foam to a slurry consisting of cementitious materials, fillers, water and various admixtures, and then mixing, pouring, and curing. Since foamed concrete contains a large number of closed pores, it has the properties of lightness, heat preservation, heat insulation, fire resistance and sound insulation. It is widely used in building wall production, thermal insulation and lining projects.
[0004] However, in the preparation process of foamed concrete, the problem of poor foam stability often occurs, which in turn affects the performance of the final foamed concrete. Therefore, there is an urgent need for a foamed concrete foaming agent that can produce highly stable foam.
[0005] Foams can be divided into two categories based on their composition. One category is the addition of surfactants to liquids, which form gas-liquid two-phase foams after stirring. This type of foam is thermodynamically unstable, so it is easily disturbed and breaks. The second category is three-phase foam, which is composed of gas-liquid-solid phases. This type of foam refers to the addition of solid particles that are insoluble in aqueous solution into the foaming agent. These solid particles can be adsorbed on the liquid film of the bubbles, which prevents gas phase transfer on the one hand and liquid film drainage on the other hand, thereby improving the stability of the foam. Nanoparticles with large specific surface area, small size and high surface activity show unique advantages in foam stabilization. Although nanoparticles show unique advantages in stabilizing foams, there are still some key scientific problems that need to be solved: high dosage of nanoparticles and high cost. Summary of the invention
[0006] In order to overcome the above problems, the present invention provides a foam concrete foaming agent based on nanoparticles and its preparation method and application. In the present invention, nano calcium silicate hydrate particles with a wetting angle of 40 to 90° are obtained by surface hydrophobic modification of nano calcium silicate hydrate. During the foaming process, the modified nano calcium silicate hydrate can be adsorbed on the gas-liquid interface, reducing surface tension, preventing liquid film rupture, and improving the stability of the foam.
[0007] In order to achieve the above technical objectives, the present invention adopts the following technical solutions:
[0008] The first aspect of the present invention provides a nanoparticle-based foam concrete foaming agent, the raw materials of which include, by weight:
[0009] 1.2-2.5 parts of anionic surfactant, 0.2-0.5 parts of thickener, 1-5 parts of modified nano calcium silicate hydrate particles, and the balance is water. The total amount of raw materials is 100 parts.
[0010] The second aspect of the present invention provides a method for preparing the above-mentioned nanoparticle-based foamed concrete foaming agent, comprising:
[0011] (1) adding a thickener to part of water according to a ratio, and mixing them evenly to obtain a thickener solution;
[0012] (2) Add anionic surfactant, thickener solution and modified nano calcium silicate hydrate particles to the remaining water in sequence under stirring, and mix them evenly to obtain a foam concrete foaming agent based on nanoparticles.
[0013] The third aspect of the present invention provides the use of the nanoparticle-based foamed concrete foaming agent in the preparation of foamed concrete.
[0014] The beneficial effects of the present invention are:
[0015] (1) In a three-phase foam system consisting of gas-liquid-solid phases, the degree of adsorption of nanoparticles on the liquid film surface will affect the stability of the foam. Hydrophilic nanoparticles mainly exist in Plato channels and only play a role in increasing the viscosity of the foaming agent, with limited effect on the stability of the foam. On the contrary, hydrophobic nanoparticles cannot play a role in stabilizing the foam, but will defoam according to the bridging-dewetting mechanism. Therefore, it is necessary to prepare nanoparticles with a suitable wetting angle, which can be adsorbed on the gas-liquid interface to improve the stability of the foam. In the present invention, the surface of nano calcium silicate hydrate is hydrophobically modified, and the silane coupling agent KH570 can react with the hydroxyl groups on the surface of the nano calcium silicate hydrate, thereby reducing the number of hydroxyl groups on the surface of the nano calcium silicate hydrate and introducing a hydrophobic organic part on the surface of the nano calcium silicate hydrate, thereby converting the hydrophilic nano calcium silicate hydrate into nano calcium silicate hydrate particles with a wetting angle of 40 to 90 degrees. In the foaming process, the modified nano calcium silicate hydrate can be adsorbed on the gas-liquid interface, thereby reducing the surface tension, preventing the liquid film from breaking, and improving the stability of the foam.
[0016] (2) Compared with ordinary foam, the foam settling distance of the foam concrete foaming agent based on nanoparticles provided in Example 2 of the present invention is reduced by 97%, the 1h water bleeding rate is reduced by 80.35%, and its stability is significantly enhanced, which fully proves that the modified nano-hydrated calcium silicate particles can be used as an effective foam stabilizer.
[0017] (3) In addition, since calcium silicate hydrate is added to foamed concrete, it acts as an early strength agent and can increase the compressive strength of concrete, thereby improving the performance of concrete. DETAILED DESCRIPTION
[0018] It should be noted that the following detailed descriptions are exemplary and are intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.
[0019] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit exemplary embodiments according to the present invention. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprising" and / or "including" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.
[0020] A first typical embodiment of the present invention provides a nanoparticle-based foam concrete foaming agent, the raw materials of which include, by weight:
[0021] 1.2-2.5 parts of anionic surfactant, 0.2-0.5 parts of thickener, 1-5 parts of modified nano calcium silicate hydrate particles, and the balance is water. The total amount of raw materials is 100 parts.
[0022] In one or more embodiments, the preparation method of the modified nano calcium silicate hydrate particles comprises:
[0023] The silane coupling agent KH570 is added to a mixed solution of ethanol and deionized water, and after mixing evenly, the pH of the mixed solution is adjusted to 4.5-5.5 to obtain a modified solution;
[0024] The nanometer calcium silicate hydrate particles are added into the modified liquid, stirred for reaction, and the solid is collected, washed and dried to obtain the modified nanometer calcium silicate hydrate particles.
[0025] Preferably, in the mixed solution of ethanol and deionized water, the volume ratio of ethanol to deionized water is 2.5-3.5:1, preferably 3:1.
[0026] Preferably, the mass fraction of the silane coupling agent KH570 in the mixed solution of ethanol and deionized water is 0.8-2%, preferably 1%.
[0027] Preferably, the mass ratio of the silane coupling agent KH570 to the nano-calcium silicate hydrate particles is 1:3-5, preferably 1:4.
[0028] Preferably, the stirring reaction speed is 450 to 600 rpm / min, preferably 500 rpm / min; the stirring reaction time is 1.5 to 3 h, preferably 2 h.
[0029] In one or more embodiments, the anionic surfactant includes one or more of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, ammonium dodecyl sulfate, triethanolamine lauryl sulfate, sodium fatty alcohol hydroxyethyl sulfonate, sodium coconut acyl methyl taurate, sodium lauryl alcohol polyoxyethylene ether carboxylate, dodecyl phosphate and disodium dodecyl alcohol polyoxyethylene ether sulfosuccinate.
[0030] In one or more embodiments, the thickener includes one or more of hydroxypropyl methylcellulose, polyvinyl alcohol cellulose, gelatin, xanthan gum, methyl cellulose and hydroxyethyl cellulose.
[0031] A second typical embodiment of the present invention provides a method for preparing the above-mentioned nanoparticle-based foamed concrete foaming agent, comprising:
[0032] (1) adding a thickener to part of water according to a ratio, and mixing them evenly to obtain a thickener solution;
[0033] (2) Add anionic surfactant, thickener solution and modified nano calcium silicate hydrate particles to the remaining water in sequence under stirring, and mix them evenly to obtain a foam concrete foaming agent based on nanoparticles.
[0034] In one or more embodiments, in order to dissolve the thickener, in step (1), the temperature of the aqueous solution can be raised to 60-100° C., and after the thickener is dissolved, the temperature is cooled to room temperature without water.
[0035] In one or more embodiments, in step (2), the stirring speed is 450-600 rpm / min, preferably 500 rpm / min.
[0036] In one or more embodiments, in step (2), after the anionic surfactant is added, the reaction is stirred for 0.5 to 2 hours, preferably 1 hour; and then the thickener solution is added.
[0037] In one or more embodiments, in step (2), after the thickener solution is ultrasonically dispersed uniformly, the modified nano-hydrated calcium silicate particles are added.
[0038] In one or more embodiments, in step (2), the modified nano-hydrated calcium silicate particles are added and stirred for reaction for 1.5 to 5 hours, preferably 2 hours.
[0039] A third typical embodiment of the present invention provides the use of the nanoparticle-based foamed concrete foaming agent in the preparation of foamed concrete.
[0040] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.
[0041] Example 1
[0042] Silane coupling agent KH570 is added to a mixed solution of ethanol and deionized water (the volume ratio of ethanol and deionized water is 3:1), and the mass fraction of silane coupling agent KH570 in the mixed solution is 1%. The pH of the mixed solution is adjusted to 5 with oxalic acid, and ultrasonic dispersion is performed for 20 minutes to obtain a modified solution. Nano-hydrated calcium silicate particles (the mass ratio of silane coupling agent KH570 to nano-hydrated calcium silicate particles is 1:4) are added to the modified solution, stirred at a speed of 500rpm / min for 2h, the solid is collected by filtration, washed with anhydrous ethanol for 3 to 4 times to remove unreacted KH570, and the solid is collected again by centrifugation, and the collected solid is dried in a drying oven at 60°C to constant weight to obtain modified nano-hydrated calcium silicate particles.
[0043] The contact angle of the modified nano-calcium silicate hydrate was measured using a contact angle meter and was 48°.
[0044] Example 2
[0045] (1) Accurately weigh 12 g of sodium dodecyl sulfate, 2.5 g of polyvinyl alcohol cellulose and 10 g of the modified nano-hydrated calcium silicate particles prepared in Example 1, and measure 970.5 mL of deionized water.
[0046] (2) Disperse polyvinyl alcohol cellulose in 200 mL of deionized water, raise the temperature of the solution to 90° C., stir at a speed of 500 rpm / min for 1 hour, and after mixing evenly, obtain a thickener solution; then cool the thickener solution to room temperature in a water-tight manner.
[0047] (3) Sodium dodecyl sulfate was dispersed in the remaining deionized water (770.8 mL), and stirred at room temperature at a speed of 500 rpm / min for 1 h. Then, the thickener solution was added and ultrasonically dispersed for 30 min. Finally, the modified nano-hydrated calcium silicate particles were added and stirred at a speed of 500 rpm / min for 2 h. After the solute was fully dissolved, a foaming agent was prepared.
[0048] Example 3
[0049] (1) Accurately weigh 12 g of triethanolamine lauryl sulfate, 3 g of methylcellulose and 20 g of the modified nano-hydrated calcium silicate particles prepared in Example 1, and measure 960 mL of deionized water.
[0050] (2) Disperse methyl cellulose in 200 mL of deionized water, raise the temperature of the solution to 80° C., stir at a speed of 500 rpm / min for 1 h, and after mixing evenly, obtain a thickener solution; then cool the thickener solution to room temperature in a water-tight manner.
[0051] (3) Triethanolamine lauryl sulfate was dispersed in the remaining deionized water (760 mL), stirred at room temperature at a speed of 500 rpm / min for 1 h, then the thickener solution was added and ultrasonically dispersed for 30 min, and finally the modified nano-hydrated calcium silicate particles were added and stirred at a speed of 500 rpm / min for 2 h. After the solute was fully dissolved, a foaming agent was prepared.
[0052] Example 4
[0053] (1) Accurately weigh 12 g of sodium lauryl polyoxyethylene ether carboxylate, 3 g of gelatin and 40 g of the modified nano-hydrated calcium silicate particles prepared in Example 1, and measure 940 mL of deionized water.
[0054] (2) Disperse gelatin in 200 mL of deionized water, raise the temperature of the solution to 80°C, stir at a speed of 500 rpm / min for 1 hour, and after mixing evenly, obtain a thickener solution; then cool the thickener solution to room temperature in a water-tight manner.
[0055] (3) Sodium lauryl polyoxyethylene ether carboxylate was dispersed in the remaining deionized water (740 mL), stirred at room temperature at a speed of 500 rpm / min for 1 h, then the thickener solution was added and ultrasonically dispersed for 30 min, and finally the modified nano-hydrated calcium silicate particles were added and stirred at a speed of 500 rpm / min for 2 h. After the solute was fully dissolved, a foaming agent was prepared.
[0056] Comparative Example 1
[0057] Ordinary foaming agent contains only sodium lauryl sulfate and water. The total amount of raw materials is 100 parts, of which sodium lauryl sulfate is 1.2 parts and the rest is water.
[0058] Comparative Example 2
[0059] Compared with Example 2, the modified nano calcium silicate hydrate particles are not added, the type of thickener is replaced by hydroxypropyl methylcellulose, and the rest is the same as Example 2.
[0060] Experimental Example 1
[0061] The foaming agents in Examples 2 to 4 and Comparative Examples 1 to 2 were subjected to foaming experiments, and the stability of the foams was compared. The test results of the 1-hour water bleeding rate, 1-hour sedimentation distance, foam half-life, and average foam diameter were calculated and are shown in Table 1 below:
[0062] Table 1 Foam stability results
[0063] Foam stability Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 1h settlement distance / mm 12 10 5 150 41 1h water seepage rate / % 7.46 4.4 0 80.35 79.6 Foam half-life / min 62 129 518 5 11 Average diameter of foam / μm 149.02 147.5 72.69 432.46 180.55
[0064] As can be seen from Table 1, compared with ordinary foam, the foam settlement distance and water penetration rate of the foam concrete foaming agent based on nanoparticles provided by the present invention are significantly reduced, the foam half-life is extended, and the average diameter of the foam is significantly reduced, proving that the foam stability of the foam concrete foaming agent based on nanoparticles provided by the present invention is significantly enhanced. At the same time, in the optimal embodiment 2, the foam settlement distance is reduced by 97%, the 1h water penetration rate is reduced by 80.35%, and its stability is significantly enhanced, which fully proves that the modified nano hydrated calcium silicate particles can be used as an effective foam stabilizer.
[0065] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A foam concrete foaming agent based on nanoparticles, characterized in that: The raw materials include by weight: 1.2-2.5 parts of anionic surfactant, 0.2-0.5 parts of thickener, 1-5 parts of modified nano-hydrated calcium silicate particles, and the balance is water, the total amount of raw materials is 100 parts; The silane coupling agent KH570 is added to a mixed solution of ethanol and deionized water, and after mixing evenly, the pH of the mixed solution is adjusted to 4.5-5.5 to obtain a modified solution; Adding nanometer calcium silicate hydrate particles into the modified liquid, stirring for reaction, collecting solids, washing, and drying to obtain modified nanometer calcium silicate hydrate particles; In the mixed solution of ethanol and deionized water, the volume ratio of ethanol to deionized water is 2.5 to 3.5:1; The mass fraction of silane coupling agent KH570 in the mixed solution of ethanol and deionized water is 0.8-2%; The mass ratio of silane coupling agent KH570 to nano calcium silicate hydrate particles is 1:3-5; The stirring reaction speed is 450-600 rpm / min; the stirring reaction time is 1.5-3h; The contact angle of the modified nano-hydrated calcium silicate is 48°; The anionic surfactant includes one or more of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, ammonium dodecyl sulfate, triethanolamine lauryl sulfate, sodium fatty alcohol hydroxyethyl sulfonate, sodium coconut acyl methyl taurate, sodium lauryl alcohol polyoxyethylene ether carboxylate, dodecyl phosphate and disodium dodecyl alcohol polyoxyethylene ether sulfosuccinate.
2. The foam concrete foaming agent according to claim 1, characterized in that In the mixed solution of ethanol and deionized water, the volume ratio of ethanol to deionized water is 3:1; Or, the mass fraction of the silane coupling agent KH570 in the mixed solution of ethanol and deionized water is 1%.
3. The foam concrete foaming agent according to claim 1, characterized in that The mass ratio of silane coupling agent KH570 to nano-calcium silicate hydrate particles is 1:
4.
4. The foam concrete foaming agent according to claim 1, characterized in that The stirring reaction speed was 500 rpm / min; the stirring reaction time was 2 h.
5. The foam concrete foaming agent according to claim 1, characterized in that The thickener includes one or more of hydroxypropyl methylcellulose, polyvinyl alcohol cellulose, gelatin, xanthan gum, methyl cellulose and hydroxyethyl cellulose.
6. The method for preparing the foamed concrete foaming agent according to any one of claims 1 to 5, characterized in that: include: (1) adding a thickener to part of water according to a ratio, and mixing them evenly to obtain a thickener solution; (2) Add anionic surfactant, thickener solution and modified nano calcium silicate hydrate particles to the remaining water in sequence under stirring, and mix them evenly to obtain a foam concrete foaming agent based on nanoparticles.
7. The preparation method according to claim 6, characterized in that: In step (1), the temperature of the aqueous solution is raised to 60-100° C., and after the thickener is dissolved, the temperature is cooled to room temperature without water; Or, in step (2), the stirring speed is 450-600 rpm / min; Or, in step (2), after adding the anionic surfactant, stirring the reaction for 0.5 to 2 hours; then adding the thickener solution; Or, in step (2), after adding the thickener solution and uniformly dispersing it by ultrasonic, the modified nano-hydrated calcium silicate particles are added; Alternatively, in step (2), the modified nano-calcium silicate hydrate particles are added and stirred to react for 1.5 to 5 hours.
8. The preparation method according to claim 6, characterized in that: In step (2), the stirring speed is 500 rpm / min; Or, in step (2), after adding the anionic surfactant, stirring the reaction for 1 hour; then adding the thickener solution; Alternatively, in step (2), the modified nano-hydrated calcium silicate particles are added and stirred to react for 2 hours.
9. Use of the foamed concrete foaming agent according to any one of claims 1 to 5 in the preparation of foamed concrete.