A kind of iron oxyhydroxide desulfurizing agent and preparation method thereof

By using porous nanosilica as a carrier and modifying it in the preparation of iron oxyhydroxide, the problems of poor performance and difficult regeneration of desulfurizers in the existing technology are solved, and efficient and stable desulfurization effects are achieved.

CN118356790BActive Publication Date: 2024-10-18DONGYING CITY HAIJIA CHEM
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410573868.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-10
Publication Date
2024-10-18
Estimated Expiration
2044-05-10

AI Technical Summary

Technical Problem

The preparation method of iron oxyhydroxide in the prior art has strict requirements on reaction conditions, and it is easy to form iron oxide compounds that cannot be regenerated, resulting in poor desulfurization performance and difficulty in regeneration.

Method used

Porous nanosilica is used as a carrier, and the iron oxyhydroxide obtained by in-situ reaction is adsorbed through specific preparation steps to improve the strength and stability of the desulfurizer, and its mechanical properties and recyclability are enhanced through modification treatment.

Benefits of technology

The prepared iron oxyhydroxide desulfurizer has high desulfurization intensity, large penetration sulfur capacity, good mechanical strength and stability, is easy to recycle, and significantly improves the desulfurization performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention proposes an iron oxyhydroxide desulfurizer and a preparation method thereof, and belongs to the technical field of desulfurizers. The invention comprises: S1. uniformly mixing tetraethyl orthosilicate, ethanol, a porogen and water, adding ammonia water to adjust the pH value, heating and stirring to react, centrifuging, washing, drying and calcining to obtain a porous silica carrier; S2. adding the porous silica carrier to ethanol, adding a silane coupling agent, heating and stirring to react, centrifuging, washing and drying to obtain a modified porous silica carrier; S3. adding the modified porous silica carrier, a soluble ferrous salt and water to molten stearic acid, heating and stirring to react in an oxygen atmosphere, and high-temperature crystallization to obtain an iron oxyhydroxide desulfurizer. The iron oxyhydroxide desulfurizer prepared by the invention uses porous nano-silica as a carrier, adsorbs the iron oxyhydroxide obtained by the in-situ reaction, has a large specific surface area of ​​the carrier, and the prepared desulfurizer has high strength, large sulfur penetration capacity, high mechanical strength, good stability, and is easy to recycle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of desulfurizing agents, and in particular to an iron oxyhydroxide desulfurizing agent and a preparation method thereof. Background Art

[0002] Iron oxyhydroxide is an important desulfurizer with broad application prospects in the fields of heavy metal particle adsorption, organic matter degradation, solid / liquid phase desulfurization and coal liquefaction. Iron oxyhydroxide can be used for desulfurization and regeneration. The reaction process is: the hydroxyl group in the iron oxyhydroxide is replaced by HS after H2S dissociation to form FeSSH for desulfurization.

[0003] After the iron oxide reaches its sulfur capacity, oxygen is introduced into it to regenerate the iron oxyhydroxide, which can then be recycled.

[0004] At present, the method for preparing ferric hydroxide is mainly wet preparation by chemical solution reaction. Since the formation of ferric hydroxide has strict requirements on reaction conditions, such as the pH value of the solution, temperature, feeding rate, etc., all of which will affect the final state of the product. Slight adjustments to the reaction environment may form non-regenerative iron oxide compounds such as ferroferric oxide, ferric oxide or crystalline ferric hydroxide during the reaction process, resulting in poor desulfurization performance of the obtained ferric hydroxide and difficulty in regeneration. Summary of the invention

[0005] The purpose of the present invention is to provide an iron oxyhydroxide desulfurizer and a preparation method thereof. The porous nano-silica is used as a carrier to adsorb the iron oxyhydroxide obtained by an in-situ reaction. The carrier has a large specific surface area, and the prepared desulfurizer has high strength, large sulfur penetration capacity, high mechanical strength, good stability, and is easy to recycle.

[0006] The technical solution of the present invention is achieved in this way:

[0007] The present invention provides a method for preparing an iron oxyhydroxide desulfurizer, comprising the following steps:

[0008] S1. Preparation of porous silica carrier: mix tetraethyl orthosilicate, ethanol, porogen and water, add ammonia water to adjust pH value, heat and stir to react, centrifuge, wash, dry and calcine to obtain porous silica carrier;

[0009] S2 modification: the porous silica carrier prepared in step S1 is added to ethanol, a silane coupling agent is added, the reaction is heated and stirred, centrifuged, washed, and dried to obtain a modified porous silica carrier;

[0010] S3. Preparation of ferric hydroxide desulfurizer: Add the modified porous silica carrier, soluble ferrous salt and water obtained in step S2 to molten stearic acid, heat and stir to react in an oxygen atmosphere, and crystallize at high temperature to obtain ferric hydroxide desulfurizer.

[0011] As a further improvement of the present invention, the mass ratio of tetraethyl orthosilicate, ethanol, porogen, water and ammonia water in step S1 is 10-12:100-120:2-4:12-15:15-20.

[0012] As a further improvement of the present invention, the temperature of the heating and stirring reaction in step S1 is 40-50°C, the time is 10-12h, and the temperature of the calcination is 500-600°C, the time is 1-2h.

[0013] As a further improvement of the present invention, the porogen in step S1 is at least one selected from the group consisting of hexadecyltrimethylammonium chloride, hexadecyldimethylbenzylammonium chloride, hexadecyldimethylbenzylammonium bromide, and hexadecyltrimethyl sodium chloride.

[0014] As a further improvement of the present invention, the mass ratio of the porous silica carrier to the silane coupling agent in step S2 is 100:12-15; the temperature of the heating and stirring reaction is 35-45° C., and the time is 0.5-1 h.

[0015] As a further improvement of the present invention, the silane coupling agent in step S2 is selected from at least one of KH550, KH560, KH570, KH580, and KH590.

[0016] As a further improvement of the present invention, the mass ratio of the modified porous silica carrier, soluble ferrous salt, water and stearic acid in step S3 is 10-12:7-12:5-7:10-15; the temperature of the heating and stirring reaction is 70-80°C, the time is 1-3h, and the temperature of the high temperature crystallization is 150-170°C, and the time is 3-5h.

[0017] As a further improvement of the present invention, the soluble ferrous salt in step S3 is selected from at least one of ferrous chloride, ferrous sulfate and ferrous nitrate.

[0018] As a further improvement of the present invention, the present invention specifically comprises the following steps:

[0019] S1. Preparation of porous silica carrier: 10-12 parts by weight of tetraethyl orthosilicate, 100-120 parts by weight of ethanol, 2-4 parts by weight of porogen, and 12-15 parts by weight of water are mixed uniformly, 15-20 parts by weight of ammonia water are added to adjust the pH value, heated to 40-50°C, stirred for 10-12h, centrifuged, washed, dried, and calcined at 500-600°C for 1-2h to obtain a porous silica carrier;

[0020] S2 modification: 100 parts by weight of the porous silica support prepared in step S1 was added to 200 parts by weight of ethanol, 12-15 parts by weight of a silane coupling agent was added, heated to 35-45 ° C, stirred for 0.5-1h, centrifuged, washed, and dried to obtain a modified porous silica support;

[0021] S3. Preparation of ferric hydroxide desulfurizer: add 10-12 parts by weight of the modified porous silica carrier obtained in step S2, 7-12 parts by weight of a soluble ferrous salt, and 5-7 parts by weight of water to 10-15 parts by weight of molten stearic acid, heat to 70-80°C in an oxygen atmosphere, stir to react for 1-3h, heat to 150-170°C, crystallize for 3-5h, and obtain the ferric hydroxide desulfurizer.

[0022] The present invention further protects an iron oxyhydroxide desulfurizing agent prepared by the above preparation method.

[0023] The present invention has the following beneficial effects: the iron oxyhydroxide desulfurizer prepared by the present invention uses porous nano-silica as a carrier, adsorbs the iron oxyhydroxide obtained by in-situ reaction, the carrier has a large specific surface area, the prepared desulfurizer has high strength, large sulfur penetration capacity, high mechanical strength, good stability, and is easy to recycle. DETAILED DESCRIPTION

[0024] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] Example 1

[0026] This embodiment provides a method for preparing an iron oxyhydroxide desulfurizer, which specifically comprises the following steps:

[0027] S1. Preparation of porous silica carrier: 10 parts by weight of tetraethyl orthosilicate, 100 parts by weight of ethanol, 2 parts by weight of hexadecyltrimethylammonium chloride, and 12 parts by weight of water were mixed evenly, 15 parts by weight of ammonia water were added to adjust the pH value, heated to 40°C, stirred for 10 hours, centrifuged, washed, dried, and calcined at 500°C for 1 hour to obtain a porous silica carrier;

[0028] S2 modification: 100 parts by weight of the porous silica carrier prepared in step S1 was added to 200 parts by weight of ethanol, 12 parts by weight of a silane coupling agent KH550 was added, heated to 35 ° C, stirred for 0.5h, centrifuged, washed, and dried to obtain a modified porous silica carrier;

[0029] S3. Preparation of ferric hydroxide desulfurizer: add 10 parts by weight of the modified porous silica carrier obtained in step S2, 7 parts by weight of ferrous chloride, and 5 parts by weight of water to 10 parts by weight of molten stearic acid, heat to 70°C in an oxygen atmosphere, stir to react for 1 hour, heat to 150°C, crystallize for 3 hours to obtain the ferric hydroxide desulfurizer.

[0030] Example 2

[0031] This embodiment provides a method for preparing an iron oxyhydroxide desulfurizer, which specifically comprises the following steps:

[0032] S1. Preparation of porous silica carrier: 12 parts by weight of tetraethyl orthosilicate, 120 parts by weight of ethanol, 4 parts by weight of hexadecyldimethylbenzyl ammonium chloride, and 15 parts by weight of water were mixed evenly, 20 parts by weight of ammonia water were added to adjust the pH value, heated to 50°C, stirred for 12 hours, centrifuged, washed, dried, and calcined at 600°C for 2 hours to obtain a porous silica carrier;

[0033] S2 modification: 100 parts by weight of the porous silica support prepared in step S1 was added to 200 parts by weight of ethanol, 15 parts by weight of a silane coupling agent KH560 was added, heated to 45 ° C, stirred for 1h, centrifuged, washed, and dried to obtain a modified porous silica support;

[0034] S3. Preparation of ferric hydroxide desulfurizer: 12 parts by weight of the modified porous silica carrier obtained in step S2, 12 parts by weight of ferrous sulfate, and 7 parts by weight of water are added to 15 parts by weight of molten stearic acid, heated to 80°C in an oxygen atmosphere, stirred for reaction for 3 hours, heated to 170°C, and crystallized for 5 hours to obtain the ferric hydroxide desulfurizer.

[0035] Example 3

[0036] This embodiment provides a method for preparing an iron oxyhydroxide desulfurizer, which specifically comprises the following steps:

[0037] S1. Preparation of porous silica carrier: 11 parts by weight of tetraethyl orthosilicate, 110 parts by weight of ethanol, 3 parts by weight of hexadecyldimethylbenzylammonium bromide, and 13 parts by weight of water were mixed evenly, 17 parts by weight of ammonia water were added to adjust the pH value, heated to 45°C, stirred for 11 hours, centrifuged, washed, dried, and calcined at 550°C for 1.5 hours to obtain a porous silica carrier;

[0038] S2 modification: 100 parts by weight of the porous silica support prepared in step S1 was added to 200 parts by weight of ethanol, 13 parts by weight of a silane coupling agent KH550 was added, heated to 40 ° C, stirred for 1 h, centrifuged, washed, and dried to obtain a modified porous silica support;

[0039] S3. Preparation of ferric hydroxide desulfurizer: 11 parts by weight of the modified porous silica carrier obtained in step S2, 10 parts by weight of ferrous nitrate, and 6 parts by weight of water are added to 12 parts by weight of molten stearic acid, heated to 75°C in an oxygen atmosphere, stirred for reaction for 2 hours, heated to 160°C, and crystallized for 4 hours to obtain the ferric hydroxide desulfurizer.

[0040] Comparative Example 1

[0041] Compared with Example 3, the difference is that the porous silica carrier prepared in step S1 is replaced by an equal mass of ZSM type molecular sieve.

[0042] The details are as follows:

[0043] S1. Modification: 100 parts by weight of ZSM molecular sieve was added to 200 parts by weight of ethanol, 13 parts by weight of silane coupling agent KH550 was added, heated to 40 ° C, stirred for 1 h, centrifuged, washed, and dried to obtain a modified ZSM molecular sieve;

[0044] S2. Preparation of ferric hydroxide desulfurizer: Add 11 parts by weight of the modified ZSM molecular sieve obtained in step S2, 10 parts by weight of ferrous nitrate, and 6 parts by weight of water to 12 parts by weight of molten stearic acid, heat to 75°C in an oxygen atmosphere, stir to react for 2 hours, heat to 160°C, crystallize for 4 hours, and obtain the ferric hydroxide desulfurizer.

[0045] Comparative Example 2

[0046] Compared with Example 3, the difference is that step S2 is not performed.

[0047] The details are as follows:

[0048] S1. Preparation of porous silica carrier: 11 parts by weight of tetraethyl orthosilicate, 110 parts by weight of ethanol, 3 parts by weight of hexadecyldimethylbenzylammonium bromide, and 13 parts by weight of water were mixed evenly, 17 parts by weight of ammonia water were added to adjust the pH value, heated to 45°C, stirred for 11 hours, centrifuged, washed, dried, and calcined at 550°C for 1.5 hours to obtain a porous silica carrier;

[0049] S2. Preparation of ferric hydroxide desulfurizer: Add 11 parts by weight of the porous silica carrier prepared in step S1, 10 parts by weight of ferrous nitrate, and 6 parts by weight of water to 12 parts by weight of molten stearic acid, heat to 75°C in an oxygen atmosphere, stir to react for 2 hours, heat to 160°C, crystallize for 4 hours, and obtain the ferric hydroxide desulfurizer.

[0050] Test Example 1

[0051] The performance of the iron oxyhydroxide desulfurizers prepared in Examples 1-3 of the present invention and Comparative Examples 1-2 was tested, and the results are shown in Table 1.

[0052] Table 1

[0053]

[0054] It can be seen from the above table that the iron oxyhydroxide desulfurizers prepared in Examples 1-3 of the present invention have better comprehensive performance.

[0055] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing an iron oxyhydroxide desulfurizer, characterized in that: The following steps are involved: S1. Preparation of porous silica carrier: mix tetraethyl orthosilicate, ethanol, porogen and water, add ammonia water to adjust pH value, heat and stir to react, centrifuge, wash, dry and calcine to obtain porous silica carrier; S2 modification: the porous silica carrier prepared in step S1 is added to ethanol, a silane coupling agent is added, the reaction is heated and stirred, centrifuged, washed, and dried to obtain a modified porous silica carrier; S3. Preparation of ferric hydroxide desulfurizer: Add the modified porous silica carrier, soluble ferrous salt and water obtained in step S2 to molten stearic acid, heat and stir to react in an oxygen atmosphere, and crystallize at high temperature to obtain ferric hydroxide desulfurizer.

2. The preparation method according to claim 1, characterized in that: The mass ratio of tetraethyl orthosilicate, ethanol, porogen, water and ammonia water in step S1 is 10-12:100-120:2-4:12-15:15-20.

3. The preparation method according to claim 1, characterized in that: The temperature of the heating and stirring reaction in step S1 is 40-50°C for 10-12 hours, and the temperature of the calcination is 500-600°C for 1-2 hours.

4. The preparation method according to claim 1, characterized in that: The porogen in step S1 is at least one selected from the group consisting of hexadecyltrimethylammonium chloride, hexadecyldimethylbenzylammonium chloride, hexadecyldimethylbenzylammonium bromide, and hexadecyltrimethyl sodium chloride.

5. The preparation method according to claim 1, characterized in that: In step S2, the mass ratio of the porous silica carrier to the silane coupling agent is 100:12-15; the temperature of the heating and stirring reaction is 35-45° C., and the time is 0.5-1 h.

6. The preparation method according to claim 1, characterized in that: The silane coupling agent in step S2 is selected from at least one of KH550, KH560, KH570, KH580, and KH590.

7. The preparation method according to claim 1, characterized in that: The mass ratio of the modified porous silica carrier, soluble ferrous salt, water and stearic acid in step S3 is 10-12:7-12:5-7:10-15; the temperature of the heating and stirring reaction is 70-80°C, the time is 1-3h, and the temperature of the high temperature crystallization is 150-170°C, and the time is 3-5h.

8. The preparation method according to claim 1, characterized in that: The soluble ferrous salt in step S3 is selected from at least one of ferrous chloride, ferrous sulfate and ferrous nitrate.

9. The preparation method according to claim 1, characterized in that: The specific steps include: S1. Preparation of porous silica carrier: 10-12 parts by weight of tetraethyl orthosilicate, 100-120 parts by weight of ethanol, 2-4 parts by weight of porogen, and 12-15 parts by weight of water are mixed uniformly, 15-20 parts by weight of ammonia water are added to adjust the pH value, heated to 40-50°C, stirred for 10-12h, centrifuged, washed, dried, and calcined at 500-600°C for 1-2h to obtain a porous silica carrier; S2 modification: 100 parts by weight of the porous silica support prepared in step S1 was added to 200 parts by weight of ethanol, 12-15 parts by weight of a silane coupling agent was added, heated to 35-45 ° C, stirred for 0.5-1h, centrifuged, washed, and dried to obtain a modified porous silica support; S3. Preparation of ferric hydroxide desulfurizer: add 10-12 parts by weight of the modified porous silica carrier obtained in step S2, 7-12 parts by weight of a soluble ferrous salt, and 5-7 parts by weight of water to 10-15 parts by weight of molten stearic acid, heat to 70-80°C in an oxygen atmosphere, stir to react for 1-3h, heat to 150-170°C, crystallize for 3-5h, and obtain the ferric hydroxide desulfurizer.

10. An iron oxyhydroxide desulfurizing agent obtained by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • High-strength FeOOH desulfurizer and preparation method thereof

    CN101584962A

  • Desulfurizing agent and preparation method thereof

    CN103301742A

  • Supported amorphous ferric hydroxide desulfurizer and preparation method thereof

    CN103418230A

  • Preparation method of FeOOH low-temperature desulfurizer and desulfurizer prepared through same

    CN105056719A

  • High-strength iron oxyhydroxide desulfurizer and preparation method thereof

    CN116212625A