A chopped carbon fiber reinforced composite material and preparation method thereof

Through the combination of chopped carbon fiber and modified dextrin and hot pressing sintering technology, the problem of poor toughness caused by uneven distribution of carbon fibers in ceramic matrix materials is solved, and the mechanical properties of ceramic matrix composite materials are significantly improved.

CN118359448BActive Publication Date: 2024-10-18TIANJIN LIGHT FUTURE TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410780464.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-10-18
Estimated Expiration
2044-06-18

AI Technical Summary

Technical Problem

The performance of existing carbon fiber reinforced ceramic matrix materials is greatly affected by the expression and distribution state of carbon fibers in the ceramic matrix, leading to the problem of poor toughness.

Method used

A combination of chopped carbon fiber, modified dextrin and dispersant is used. Through coupling agent treatment and hot pressing sintering method, a combination of modified chopped carbon fiber and ceramic slurry precursor is formed to improve the mechanical strength and interface bonding of the material.

Benefits of technology

Through the close combination of modified chopped carbon fiber and ceramic slurry, the mechanical properties of the composite material are significantly improved and the overall performance of the material is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention provides a chopped carbon fiber reinforced composite material and a preparation method thereof, the method comprising the following steps: mixing silicon carbide powder, silicon nitride powder and a sintering aid and dissolving them in ethanol to obtain a ceramic slurry precursor; mixing the treated chopped carbon fiber with modified dextrin and a dispersant and standing to obtain the modified chopped carbon fiber; mixing chopped carbon fiber II, the modified chopped carbon fiber and the ceramic slurry precursor and pouring them into a mold, hot pressing and sintering to obtain the chopped carbon fiber reinforced composite material. The chopped carbon fiber reinforced composite material of the invention enhances the mechanical strength of the material itself by combining modified chopped carbon fiber, ordinary chopped carbon fiber and ceramic slurry precursor; in the modified chopped carbon fiber, the modified dextrin is coated on the outside of the chopped carbon fiber treated with a coupling agent, and the modified dextrin has a unique hydrophilic structure, so that the modified chopped carbon fiber is tightly combined with the ceramic slurry and the chopped carbon fiber.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of composite materials, and in particular relates to a chopped carbon fiber reinforced composite material and a preparation method thereof. Background Art

[0002] Ceramic materials have excellent comprehensive properties, including high specific stiffness, high strength and good chemical inertness. At the same time, ceramic materials also have the advantages of low density, high hardness and high compressive strength. The excellent properties of ceramic materials make their application in the field of aeroengines very promising.

[0003] Carbon fiber is compounded with ceramic-based materials. By reinforcing ceramic-based materials with carbon fiber, the disadvantage of poor toughness of ceramic-based materials can be improved. Carbon fiber can strengthen ceramics through surface modification. However, for carbon fiber reinforced ceramic-based materials, the form and distribution of carbon fiber in the ceramic matrix seriously affect the performance of ceramic-based composite materials. Summary of the invention

[0004] In view of this, the present invention aims to overcome the defects in the prior art and proposes a chopped carbon fiber reinforced composite material and a preparation method thereof.

[0005] To achieve the above object, the technical solution of the present invention is achieved as follows:

[0006] A method for preparing a chopped carbon fiber reinforced composite material comprises the following steps:

[0007] Step 1 is to mix silicon carbide powder, silicon nitride powder and a sintering aid and dissolve them in deionized water to obtain a ceramic slurry precursor;

[0008] Step 2 is to mix the treated chopped carbon fiber with modified dextrin and a dispersant, and let stand to obtain modified chopped carbon fiber;

[0009] Step 3 is to mix the chopped carbon fiber II, the modified chopped carbon fiber and the ceramic slurry precursor, pour them into a mold, and obtain the chopped carbon fiber reinforced composite material after hot pressing and sintering.

[0010] Furthermore, the mass ratio of silicon carbide powder, silicon nitride powder and sintering aid in step 1 is 50-99:1-30:0.1-10; the sintering aid is at least one of magnesium oxide, calcium oxide, yttrium oxide, lanthanum oxide or praseodymium oxide.

[0011] Preferably, the mass ratio of silicon carbide powder, silicon nitride powder and sintering aid in step 1 is 50-80:1-30:0.1-5.

[0012] Furthermore, the treated short-cut carbon fiber in step 2 is prepared by a method comprising the following steps: adding a coupling agent to a solvent, mixing uniformly, adding short-cut carbon fiber I thereto, heating and reacting, and obtaining the treated short-cut carbon fiber. The coupling agent acts as an intermediate transition layer to improve the interface polarity and compatibility, and promotes the uniform coating of the modified dextrin on the surface of the short-cut carbon fiber, and the interface bonding is good.

[0013] Furthermore, the coupling agent is at least one of vinyl triethoxysilane, methacryloxysilane or aminopropyl triethoxysilane; the solvent is an ethanol solution with a mass concentration of 30-70%; the temperature of the heating step is 60-80°C; the solid-liquid ratio of the chopped carbon fiber I, the coupling agent and the solvent is 10-30g:0.1-1g:100mL; the length of the chopped carbon fiber I is 15-20 mm and the diameter is 10-15 microns. The chopped carbon fiber I is made by crushing carbon fiber filaments.

[0014] Furthermore, the modified dextrin in step 2 is prepared by a method comprising the following steps: nitrogen is introduced into a dextrin solution, propylene oxide and sodium hydroxide are added thereto, and the modified dextrin is obtained after reaction.

[0015] Furthermore, the mass concentration of the dextrin solution is 30-60%; the mass ratio of the dextrin solution, propylene oxide and sodium hydroxide is 100:0.1-5:0.01-1; and the time of the reaction step is 0.5-48 hours.

[0016] Hydroxypropyl β-cyclodextrin is produced by passing nitrogen into the dextrin solution and adding propylene oxide and sodium hydroxide. The hydroxyl groups are distributed on the outer edge of the cavity of the hydroxypropyl β-cyclodextrin molecule, making it hydrophilic; the inner cavity of hydroxy β-cyclodextrin is composed of hydrogen atoms on carbon atoms at positions 3 and 5 and oxygen atoms on carbon atoms at position 4, showing relative hydrophobicity. Therefore, hydroxypropyl β-cyclodextrin has a special cavity structure that is hydrophilic on the outside and hydrophobic on the inside.

[0017] Furthermore, the mass ratio of the treated chopped carbon fibers to the modified dextrin and the dispersant in step 2 is 1:0.1-10:0.01-1; the dispersant is at least one of tetramethylammonium hydroxide, polyacrylic acid or polyethylene glycol.

[0018] Preferably, the mass ratio of the treated chopped carbon fibers to the modified dextrin and the dispersant in step 2 is 1:0.1-2:0.01-0.2.

[0019] Furthermore, the mass ratio of the chopped carbon fiber II in step 3, the modified chopped carbon fiber and the ceramic slurry precursor is 1-50:1-50:100; the length of the chopped carbon fiber II is 1-10 mm and the diameter is 4-8 μm. The chopped carbon fiber II is made by crushing carbon fiber filaments. The raw materials of the chopped carbon fiber I and the chopped carbon fiber II are the same, and the difference lies in their length and diameter.

[0020] Preferably, the mass ratio of the chopped carbon fiber II in step 3, the modified chopped carbon fiber and the ceramic slurry precursor is 1-5:1-10:100.

[0021] A chopped carbon fiber reinforced composite material prepared by using the preparation method.

[0022] Compared with the prior art, the present invention has the following advantages:

[0023] The chopped carbon fiber reinforced composite material of the present invention enhances the mechanical strength of the material itself by combining modified chopped carbon fibers, ordinary chopped carbon fibers and a ceramic slurry precursor; in the modified chopped carbon fibers, modified dextrin is coated on the outside of the chopped carbon fibers treated with a coupling agent, and the unique hydrophilic structure of the modified dextrin makes the modified chopped carbon fibers, the ceramic slurry and the chopped carbon fibers more tightly combined, thereby further improving the performance of the composite material. DETAILED DESCRIPTION

[0024] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.

[0025] The present invention will be described in detail below with reference to the embodiments.

[0026] Example 1

[0027] A method for preparing a chopped carbon fiber reinforced composite material comprises the following steps:

[0028] (1) 60 parts of silicon carbide powder, 20 parts of silicon nitride powder and 5 parts of yttrium oxide were mixed and dissolved in 2 times the amount of deionized water, and then ball-milled and sieved to obtain a ceramic slurry precursor;

[0029] (2) Add 0.1 g of aminopropyltriethoxysilane to 100 ml of 60% ethanol solution, mix well, add 20 g of chopped carbon fiber I therein, and heat at 70°C for reaction to obtain treated chopped carbon fiber;

[0030] (3) nitrogen was introduced into 100 g of 30% dextrin solution, 2 g of propylene oxide and 0.5 g of sodium hydroxide were added thereto, and the solution was reacted for 48 hours to obtain the modified dextrin;

[0031] (4) mixing 100 g of the treated chopped carbon fiber with 100 g of modified dextrin and 1 g of a dispersant, and letting the mixture stand to obtain modified chopped carbon fiber;

[0032] (5) Mix 1 part of chopped carbon fiber II, 3 parts of modified chopped carbon fiber and 100 parts of ceramic slurry precursor, pour them into a mold, and then hot press and sinter at 1500° C. to obtain the chopped carbon fiber reinforced composite material.

[0033] Example 2

[0034] A method for preparing a chopped carbon fiber reinforced composite material comprises the following steps:

[0035] (1) 60 parts of silicon carbide powder, 20 parts of silicon nitride powder and 5 parts of yttrium oxide were mixed and dissolved in 2 times the amount of deionized water, and then ball-milled and sieved to obtain a ceramic slurry precursor;

[0036] (2) Add 0.1 g of aminopropyltriethoxysilane to 100 ml of 60% ethanol solution, mix well, add 20 g of chopped carbon fiber I therein, and heat at 70°C for reaction to obtain treated chopped carbon fiber;

[0037] (3) nitrogen was introduced into 100 g of 30% dextrin solution, 2 g of propylene oxide and 0.5 g of sodium hydroxide were added thereto, and the solution was reacted for 48 hours to obtain the modified dextrin;

[0038] (4) mixing 100 g of the treated chopped carbon fiber with 100 g of modified dextrin and 1 g of a dispersant, and letting the mixture stand to obtain modified chopped carbon fiber;

[0039] (5) 2 parts of chopped carbon fiber II, 2 parts of modified chopped carbon fiber and 100 parts of ceramic slurry precursor are mixed and poured into a mold, and then hot pressed and sintered at 1500° C. to obtain the chopped carbon fiber reinforced composite material.

[0040] Comparative Example 1

[0041] A method for preparing a chopped carbon fiber reinforced composite material comprises the following steps:

[0042] (1) 60 parts of silicon carbide powder, 20 parts of silicon nitride powder and 5 parts of yttrium oxide were mixed and dissolved in 2 times the amount of deionized water, and then ball-milled and sieved to obtain a ceramic slurry precursor;

[0043] (2) nitrogen was introduced into 100 g of 30% dextrin solution, 2 g of propylene oxide and 0.5 g of sodium hydroxide were added thereto, and the solution was reacted for 48 hours to obtain the modified dextrin;

[0044] (3) 100 g of chopped carbon fiber I, 100 g of modified dextrin, and 1 g of a dispersant were mixed and allowed to stand to obtain modified chopped carbon fiber;

[0045] (4) 1 part of chopped carbon fiber II, 3 parts of modified chopped carbon fiber and 100 parts of ceramic slurry precursor are mixed and poured into a mold, and then hot pressed and sintered at 1500° C. to obtain the chopped carbon fiber reinforced composite material.

[0046] Comparative Example 2

[0047] A method for preparing a chopped carbon fiber reinforced composite material comprises the following steps:

[0048] (1) 60 parts of silicon carbide powder, 20 parts of silicon nitride powder and 5 parts of yttrium oxide were mixed and dissolved in 2 times the amount of deionized water, and then ball-milled and sieved to obtain a ceramic slurry precursor;

[0049] (2) Add 0.1 g of aminopropyltriethoxysilane to 100 ml of 60% ethanol solution, mix well, add 20 g of chopped carbon fiber I therein, and heat at 70°C for reaction to obtain treated chopped carbon fiber;

[0050] (3) Mixing 100 g of the treated chopped carbon fiber with 100 g of dextrin solution and 1 g of a dispersant, and letting the mixture stand to obtain modified chopped carbon fiber;

[0051] (4) 1 part of chopped carbon fiber II, 3 parts of modified chopped carbon fiber and 100 parts of ceramic slurry precursor are mixed and poured into a mold, and then hot pressed and sintered at 1500° C. to obtain the chopped carbon fiber reinforced composite material.

[0052] Comparative Example 3

[0053] A method for preparing a chopped carbon fiber reinforced composite material comprises the following steps:

[0054] (1) 60 parts of silicon carbide powder, 20 parts of silicon nitride powder and 5 parts of yttrium oxide were mixed and dissolved in 2 times the amount of deionized water, and then ball-milled and sieved to obtain a ceramic slurry precursor;

[0055] (2) 100 g of chopped carbon fiber I was mixed with 100 g of dextrin solution and 1 g of dispersant, and the mixture was allowed to stand to obtain modified chopped carbon fiber;

[0056] (3) Mix 1 part of chopped carbon fiber II, 3 parts of modified chopped carbon fiber and 100 parts of ceramic slurry precursor, pour them into a mold, and then hot press and sinter at 1500° C. to obtain the chopped carbon fiber reinforced composite material.

[0057] Comparative Example 4

[0058] A method for preparing a chopped carbon fiber reinforced composite material comprises the following steps:

[0059] (1) 60 parts of silicon carbide powder, 20 parts of silicon nitride powder and 5 parts of yttrium oxide were mixed and dissolved in 2 times the amount of deionized water, and then ball-milled and sieved to obtain a ceramic slurry precursor;

[0060] (2) Mix 1 part of chopped carbon fiber II, 3 parts of chopped carbon fiber I and 100 parts of ceramic slurry precursor, pour them into a mold, and then hot press and sinter at 1500° C. to obtain the chopped carbon fiber reinforced composite material.

[0061] Comparative Example 5

[0062] A method for preparing a chopped carbon fiber reinforced composite material comprises the following steps:

[0063] (1) 60 parts of silicon carbide powder, 20 parts of silicon nitride powder and 5 parts of yttrium oxide were mixed and dissolved in 2 times the amount of deionized water, and then ball-milled and sieved to obtain a ceramic slurry precursor;

[0064] (2) 4 parts of chopped carbon fiber II and 100 parts of ceramic slurry precursor are mixed and poured into a mold, and then hot-pressed and sintered at 1500° C. to obtain the chopped carbon fiber reinforced composite material.

[0065] The mechanical properties of the products obtained in Examples 1-2 and Comparative Examples 1-5 are shown in Table 1. The results are shown in Table 1.

[0066] Table 1 Test results

[0067]

[0068] It can be seen from Table 1 that the composite materials obtained in Examples 1-2 have excellent mechanical properties; in Comparative Example 1, the chopped carbon fiber I was not treated, and was directly modified with the modified dextrin, which affected the combination of the chopped carbon fiber I and the modified dextrin, thereby affecting the performance of the composite material; in Comparative Example 2, the dextrin was not modified, resulting in the dextrin solution only being able to reflect partial adhesion in the system, and failing to improve the overall performance of the modified chopped carbon fiber; in Comparative Example 3, chopped carbon fiber I and dextrin were directly used, lacking cross-linking, which affected the overall composite material; Comparative Example 4 directly used chopped carbon fiber II and chopped carbon fiber I, and carbon fibers of different lengths and diameters were mixed and used, which brought certain effects to the composite material compared to the use of a single size of chopped carbon fiber in Comparative Example 5.

[0069] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a chopped carbon fiber reinforced composite material, characterized in that: The steps include: Step 1 is to mix silicon carbide powder, silicon nitride powder and a sintering aid and dissolve them in deionized water to obtain a ceramic slurry precursor; Step 2 is to mix the treated chopped carbon fiber with modified dextrin and a dispersant, and let stand to obtain modified chopped carbon fiber; Step 3 is to mix the chopped carbon fiber II, the modified chopped carbon fiber and the ceramic slurry precursor, pour them into a mold, and obtain the chopped carbon fiber reinforced composite material after hot pressing and sintering; The mass ratio of silicon carbide powder, silicon nitride powder and sintering aid in step 1 is 50-99:1-30:0.1-10; The treated chopped carbon fibers in step 2 are prepared by a method comprising the following steps: adding a coupling agent to a solvent, mixing the mixture evenly, adding chopped carbon fibers I thereto, and heating the mixture for reaction to obtain treated chopped carbon fibers; The chopped carbon fiber I has a length of 15-20 mm and a diameter of 10-15 μm; The modified dextrin in step 2 is prepared by a method comprising the following steps: introducing nitrogen into a dextrin solution, adding propylene oxide and sodium hydroxide thereto, and obtaining the modified dextrin after reaction; The mass concentration of the dextrin solution is 30-60%; the mass ratio of the dextrin solution, propylene oxide and sodium hydroxide is 100:0.1-5:0.01-1; the time of the reaction step is 0.5-48 hours; The mass ratio of the chopped carbon fiber II in step 3, the modified chopped carbon fiber and the ceramic slurry precursor is 1-5:1-10:

100.

2. The method for preparing a chopped carbon fiber reinforced composite material according to claim 1, characterized in that: The sintering aid is at least one of magnesium oxide, calcium oxide, yttrium oxide, lanthanum oxide or praseodymium oxide.

3. The method for preparing a chopped carbon fiber reinforced composite material according to claim 1, characterized in that: The coupling agent is at least one of vinyl triethoxysilane, methacryloxysilane or aminopropyl triethoxysilane; the solvent is an ethanol solution with a mass concentration of 30-70%; the temperature of the heating step is 60-80°C; the solid-liquid ratio of the chopped carbon fiber I, the coupling agent and the solvent is 10-30g:0.1-1g:100mL.

4. The method for preparing a chopped carbon fiber reinforced composite material according to claim 1, characterized in that: The mass ratio of the treated chopped carbon fibers to the modified dextrin and the dispersant in step 2 is 1:0.1-10:0.01-1; the dispersant is at least one of tetramethylammonium hydroxide, polyacrylic acid or polyethylene glycol.

5. A chopped carbon fiber reinforced composite material prepared by the preparation method according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Toughened silicon nitride combined silicon carbide ceramic composite material and preparation method thereof