A polystyrene composite material and preparation method thereof

By adding modified monomers and flame-retardant fillers to polystyrene materials to form coordination and grafting structures, the problems of polystyrene materials being easy to break and burn are solved, and its mechanical properties and flame-retardant properties are improved.

CN118359774BActive Publication Date: 2024-10-22DONGGUAN CITY BAOHUA PLASTIC MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410291757.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-14
Publication Date
2024-10-22
Estimated Expiration
2044-03-14

AI Technical Summary

Technical Problem

Polystyrene materials are prone to breakage or stress cracking when impacted, and are easy to burn, making them unable to meet market demands for their mechanical properties.

Method used

By reacting the modified monomer, styrene and DMF under the action of azobisisobutyronitrile, and adding zinc nitrate hexahydrate and flame retardant fillers, a coordination and grafting structure is formed to improve the mechanical properties and resistance of the material. combustion performance.

Benefits of technology

It improves the mechanical properties and durability of polystyrene composite materials, inhibits heat and mass transfer during combustion, produces metal oxides to increase the density of the carbon layer, reduces the concentration of combustible gases, and achieves flame retardant effects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004740946440000111
    Figure BDA0004740946440000111
Patent Text Reader

Abstract

The invention discloses a polystyrene composite material and a preparation method thereof. After a modified monomer and styrene are reacted under the action of azobisisobutyronitrile, hexahydrate zinc nitrate and a flame retardant filler are added, the pyridine group on the modified monomer can form coordination with zinc ions, and the boric acid group on the modified monomer can be grafted with a hydroxyl group on the surface of the flame retardant filler, and finally the composite material is fully polymerized. The coordination between the pyridine group and the zinc ion can increase the mechanical properties of the composite material, and the material has a certain self-repairing property. During combustion, metal oxides can be generated to increase the compactness of the carbon layer and inhibit heat and mass transfer. Ammonium polyphosphate and organic phosphorus can generate polyphosphoric acid, pyrophosphoric acid and metaphosphoric acid to react with a substrate to form a carbon layer for protection. The modified monomer contains B, N and Si elements to increase the compactness of the carbon layer, and generates non-flammable gases such as nitric oxide and ammonia, thereby reducing the concentration of the combustible gas and taking away the heat generated by combustion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite material preparation, and in particular to a polystyrene composite material and a preparation method thereof. Background Art

[0002] Polystyrene is a polymer formed by free radical polymerization of St monomers. It is a lightweight particle with low apparent density, light weight, low thermal conductivity, low water absorption, easy processing, and low price. In addition, it has the advantages of corrosion resistance, water resistance, good electrical insulation, and easy coloring. Due to its good melt thermal stability and fluidity, it is easy to process and shape, especially easy to injection mold, suitable for production and application, and has been widely used in the fields of household appliances, instruments and meters, electronic products, automotive interior parts, and packaging materials. However, polystyrene itself has poor toughness, and its mechanical properties such as bending strength and impact strength cannot meet the market demand, which leads to consumers' concerns about the use of polystyrene materials, which in turn limits the application and development of polystyrene insulation boards to a large extent. Therefore, it is necessary to modify the polystyrene matrix. Summary of the invention

[0003] The purpose of the present invention is to provide a polystyrene composite material and a preparation method thereof, which solves the problem that the current polystyrene material is easily broken or stress cracked when impacted and is easy to burn.

[0004] The purpose of the present invention can be achieved through the following technical solutions:

[0005] A method for preparing a polystyrene composite material comprises the following steps:

[0006] The modified monomer, styrene and DMF are mixed evenly, stirred and azobisisobutyronitrile is added at a speed of 60-80r / min and a temperature of 75-80°C, reacted for 1-2h, zinc nitrate hexahydrate and flame retardant filler are added, the reaction is continued for 3-5h, filtered and dried to obtain a polystyrene composite material.

[0007] Furthermore, the mass ratio of the modified monomer, propylene, zinc nitrate hexahydrate and flame retardant filler is 15:50:3:2, and the amount of azobisisobutyronitrile is 1% of the mass of the modified monomer.

[0008] Further, the modified monomer is prepared by the following steps:

[0009] Step A1: 2,6-diaminopyridine, 3-glycidyloxypropyldimethylmethoxysilane and DMF are mixed evenly, and the mixture is reacted for 6-8 hours at a speed of 150-200 r / min, a temperature of 40-50° C. and a pH value of 10-11 to obtain intermediate 1; 4-vinylbenzoic acid, intermediate 1, p-toluenesulfonic acid and DMF are mixed evenly, and the mixture is reacted for 8-10 hours at a speed of 120-150 r / min and a temperature of 110-120° C. to obtain intermediate 2;

[0010] Step A2: Mix the intermediate 2, diphenyldichlorosilane and deionized water, stir for 10-15 minutes at a speed of 200-300 r / min and a temperature of 60-70° C., add concentrated sulfuric acid and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, react for 4-6 hours, and adjust the pH to neutral to obtain a diamine-terminated polysiloxane;

[0011] Step A3: Mix the diamine-terminated polysiloxane, 4-formylphenylboronic acid and DMF evenly, stir for 2-3 hours at a rotation speed of 150-200 r / min and a temperature of 60-65° C. to obtain intermediate 3, mix the intermediate 3, anhydrous sodium sulfate and DMF evenly, react at a temperature of 50-55° C. under a nitrogen atmosphere for 20-25 hours to obtain a modified monomer.

[0012] Furthermore, the molar ratio of 2,6-diaminopyridine and 3-glycidyloxypropyldimethylmethoxysilane in step A1 is 1:2, the molar ratio of intermediate 1 and 4-vinylbenzoic acid is 1:2, and the amount of p-toluenesulfonic acid is 1-1.5% of the mass of 4-vinylbenzoic acid.

[0013] Furthermore, the amount ratio of the intermediate 2, diphenyldichlorosilane, deionized water and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane described in step A2 is 5 mmol:2 mmol:20 mL:5 mmol, and the amount of concentrated sulfuric acid is 2% of the mass of the intermediate 1.

[0014] Furthermore, the molar ratio of the diamine-terminated polysiloxane to 4-formylphenylboronic acid in step A3 is 1:2, and the molar ratio of the intermediate 3 to anhydrous sodium sulfate is 1.3:4.2.

[0015] Furthermore, the flame retardant filler is prepared by the following steps:

[0016] Step B1: 2,2'-dihydroxybiphenyl and concentrated sulfuric acid are mixed, stirred and nitric acid solution is added dropwise at a speed of 60-120 r / min and a temperature of 20-25°C, and the reaction is carried out for 3-5 hours, and then the mixture is cooled in an ice water bath, and the filtrate is removed by filtration to obtain intermediate 4; intermediate 4, tin and concentrated hydrochloric acid are mixed, and the mixture is refluxed for 1-1.5 hours at a speed of 150-200 r / min and a temperature of 110-120°C, and concentrated ammonia water is added to adjust the pH value to 8, the mixture is boiled in water for 20-30 minutes, and the residue is removed by filtration, and glacial vinegar is added to the filtrate to adjust the pH value to 4, and the filtrate is removed by filtration to obtain a modifier;

[0017] Step B2: Evenly mix terephthalaldehyde, modifier and ethyl acetate, stir for 2-3h at a speed of 150-200r / min and a temperature of 60-65°C, then add DOPO and methanol, cool to 20-25°C, continue to react for 20-25h to obtain a treating agent, dissolve the treating agent in ethyl acetate, introduce nitrogen protection, stir and add ammonium polyphosphate at a speed of 150-200r / min and a temperature of 20-25°C, raise the temperature to 65-70°C, react for 4-5h, raise the temperature to 80-85°C, keep warm and dry to obtain a flame retardant filler.

[0018] Furthermore, the amount ratio of 2,2'-dihydroxybiphenyl, concentrated sulfuric acid and nitric acid solution in step B1 is 0.02mol:50mL:15mL, the mass fraction of concentrated sulfuric acid is 98%, the mass fraction of nitric acid solution is 50%, the amount ratio of intermediate 4, tin and concentrated hydrochloric acid is 3g:8g:20mL, and the mass fraction of concentrated hydrochloric acid is 36%.

[0019] Furthermore, the molar ratio of terephthalaldehyde, modifier and DOPO in step B2 is n:n+1:2n, n is a natural number greater than 0, and the mass ratio of the treating agent to ammonium polyphosphate is 3.5:5.

[0020] Beneficial effects of the present invention: A polystyrene composite material prepared by the present invention comprises the following steps: after a modified monomer and styrene are reacted under the action of azobisisobutyronitrile, hexahydrate zinc nitrate and a flame retardant filler are added, the pyridine group on the modified monomer can form a coordination with the zinc ion, and the boric acid group on the modified monomer can be grafted with the hydroxyl group on the surface of the flame retardant filler, and finally the polystyrene composite material is obtained by fully polymerizing, the coordination between the pyridine group and the zinc ion can increase the mechanical properties of the composite material, and at the same time, the material has a certain self-healing property, and during combustion, metal oxides can be generated to increase the compactness of the carbon layer and inhibit heat and mass transfer, the modified monomer is 2,6-diaminopyridine and 3 -glycidyloxypropyl dimethylmethoxysilane as a raw material, under alkaline conditions, the amino group on 2,6-diaminopyridine reacts with the epoxy group on 3-glycidyloxypropyl dimethylmethoxysilane to form a hydroxyl group to obtain intermediate 1, intermediate 1 is esterified with 4-vinylbenzoic acid, so that the hydroxyl group on intermediate 1 reacts with the carboxyl group on 4-vinylbenzoic acid to obtain intermediate 2, intermediate 2 and diphenyldichlorosilane are hydrolyzed, and then polymerized with 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane to form a diamine-terminated polysiloxane, and the diamine-terminated polysiloxane is reacted with 4-formylphenylboronic acid to react the amino group on the diamine-terminated polysiloxane with 4-methylboronic acid. The aldehyde group on the acylphenylboronic acid is reacted to obtain intermediate 3, and intermediate 3 is subjected to the action of anhydrous sodium sulfate to form a hexacyclic dynamic cross-linked network of boron to obtain a modified monomer. The modified monomer molecule contains a BO hexacyclic dynamic cross-linked network structure, which can greatly improve the mechanical properties of the material when combined with the metal coordination bond. At the same time, after being damaged by excessive impact, it can self-repair through dynamic bonds, thereby increasing the durability of the material. The molecular chain contains organic silicon segments and hyperbranched structures, which further improve the mechanical properties of the material. The flame retardant filler uses 2,2'-dihydroxybiphenyl as a raw material. Under the action of nitric acid solution, the grafted nitro group on the benzene ring is reduced with metal tin to make the nitric acid The aldehyde group on the terephthalaldehyde is converted into an amino group to obtain a modifier, and the terephthalaldehyde and the modifier are reacted to make the aldehyde group on the terephthalaldehyde react with the amino group on the modifier to form a C=N bond, and the C=N bond reacts with the PH bond on the DOPO to obtain a treating agent, and the treating agent and ammonium polyphosphate are subjected to an ion exchange reaction to make the treating agent coated on the surface of the ammonium polyphosphate to obtain a flame retardant filler. During combustion, the ammonium polyphosphate and organic phosphorus can produce polyphosphoric acid, pyrophosphoric acid and metaphosphoric acid to react with the substrate to form a carbon layer protection, and the modified monomer contains B, N and Si elements to increase the density of the carbon layer, and produces non-flammable gases such as nitric oxide and ammonia, which reduce the concentration of the combustible gas and take away the heat generated by the combustion, thereby achieving a flame retardant effect. DETAILED DESCRIPTION

[0021] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0022] Example 1

[0023] A method for preparing a polystyrene composite material comprises the following steps:

[0024] The modified monomer, styrene and DMF were mixed evenly, stirred and azobisisobutyronitrile was added at a speed of 60 r / min and a temperature of 75°C, reacted for 1 hour, zinc nitrate hexahydrate and flame retardant filler were added, the reaction was continued for 3 hours, filtered and dried to obtain a polystyrene composite material.

[0025] The mass ratio of the modified monomer, propylene, zinc nitrate hexahydrate and flame retardant filler is 15:50:3:2, and the amount of azobisisobutyronitrile is 1% of the mass of the modified monomer.

[0026] The modified monomer is prepared by the following steps:

[0027] Step A1: 2,6-diaminopyridine, 3-glycidyloxypropyldimethylmethoxysilane and DMF were mixed evenly, and the mixture was reacted for 6 hours at a speed of 150 r / min, a temperature of 40° C. and a pH of 10 to obtain intermediate 1; 4-vinylbenzoic acid, intermediate 1, p-toluenesulfonic acid and DMF were mixed evenly, and the mixture was reacted for 8 hours at a speed of 120 r / min and a temperature of 110° C. to obtain intermediate 2;

[0028] Step A2: Intermediate 2, diphenyldichlorosilane and deionized water were mixed, stirred for 10 min at a speed of 200 r / min and a temperature of 60° C., concentrated sulfuric acid and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane were added, and the mixture was reacted for 4 h, and the pH was adjusted to neutral to obtain a diamine-terminated polysiloxane;

[0029] Step A3: Mix the diamine-terminated polysiloxane, 4-formylphenylboronic acid and DMF evenly, stir for 2 h at a speed of 150 r / min and a temperature of 60°C to obtain intermediate 3, mix the intermediate 3, anhydrous sodium sulfate and DMF evenly, react at a temperature of 50°C under a nitrogen atmosphere for 20 h to obtain a modified monomer.

[0030] The molar ratio of 2,6-diaminopyridine and 3-glycidyloxypropyldimethylmethoxysilane in step A1 is 1:2, the molar ratio of intermediate 1 and 4-vinylbenzoic acid is 1:2, and the amount of p-toluenesulfonic acid used is 1% of the mass of 4-vinylbenzoic acid.

[0031] The amount ratio of intermediate 2, diphenyldichlorosilane, deionized water and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane described in step A2 is 5 mmol:2 mmol:20 mL:5 mmol, and the amount of concentrated sulfuric acid is 2% of the mass of intermediate 1.

[0032] The molar ratio of the diamine-terminated polysiloxane to 4-formylphenylboronic acid in step A3 is 1:2, and the molar ratio of the intermediate 3 to anhydrous sodium sulfate is 1.3:4.2.

[0033] The flame retardant filler is prepared by the following steps:

[0034] Step B1: 2,2'-dihydroxybiphenyl and concentrated sulfuric acid are mixed, stirred and nitric acid solution is added dropwise at a speed of 60 r / min and a temperature of 20°C, and the mixture is reacted for 3 hours, cooled in an ice water bath, and the filtrate is removed by filtration to obtain intermediate 4; intermediate 4, tin and concentrated hydrochloric acid are mixed, and refluxed for 1 hour at a speed of 150 r / min and a temperature of 110°C, and concentrated ammonia water is added to adjust the pH value to 8, the mixture is boiled for 20 minutes, and the residue is removed by filtration, and glacial vinegar is added to the filtrate to adjust the pH value to 4, and the filtrate is removed by filtration to obtain a modifier;

[0035] Step B2: Evenly mix terephthalaldehyde, modifier and ethyl acetate, stir for 2 hours at a speed of 150 r / min and a temperature of 60°C, then add DOPO and methanol, cool to 20°C, and continue to react for 20 hours to obtain a treating agent, dissolve the treating agent in ethyl acetate, introduce nitrogen protection, stir and add ammonium polyphosphate at a speed of 150 r / min and a temperature of 20°C, heat to 65°C, react for 4 hours, heat to 80°C, keep warm and dry to obtain a flame retardant filler.

[0036] The amount ratio of 2,2'-dihydroxybiphenyl, concentrated sulfuric acid and nitric acid solution in step B1 is 0.02 mol:50 mL:15 mL, the mass fraction of concentrated sulfuric acid is 98%, the mass fraction of nitric acid solution is 50%, the amount ratio of intermediate 4, tin and concentrated hydrochloric acid is 3 g:8 g:20 mL, and the mass fraction of concentrated hydrochloric acid is 36%.

[0037] The molar ratio of terephthalaldehyde, modifier and DOPO in step B2 is 1:2:2, and the mass ratio of treating agent and ammonium polyphosphate is 3.5:5.

[0038] Example 2

[0039] A method for preparing a polystyrene composite material comprises the following steps:

[0040] The modified monomer, styrene and DMF were mixed evenly, stirred and azobisisobutyronitrile was added at a speed of 60 r / min and a temperature of 78°C, and reacted for 2 hours. Then, zinc nitrate hexahydrate and flame retardant filler were added, and the reaction was continued for 4 hours. The mixture was filtered and dried to obtain a polystyrene composite material.

[0041] The mass ratio of the modified monomer, propylene, zinc nitrate hexahydrate and flame retardant filler is 15:50:3:2, and the amount of azobisisobutyronitrile is 1% of the mass of the modified monomer.

[0042] The modified monomer is prepared by the following steps:

[0043] Step A1: 2,6-diaminopyridine, 3-glycidyloxypropyldimethylmethoxysilane and DMF were mixed evenly, and the mixture was reacted for 7 hours at a speed of 150 r / min, a temperature of 45° C. and a pH value of 10 to obtain intermediate 1; 4-vinylbenzoic acid, intermediate 1, p-toluenesulfonic acid and DMF were mixed evenly, and the mixture was reacted for 9 hours at a speed of 120 r / min and a temperature of 115° C. to obtain intermediate 2;

[0044] Step A2: Intermediate 2, diphenyldichlorosilane and deionized water were mixed, stirred for 15 min at a speed of 200 r / min and a temperature of 65° C., concentrated sulfuric acid and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane were added, and the reaction was carried out for 5 h. The pH was adjusted to neutral to obtain a diamine-terminated polysiloxane;

[0045] Step A3: Mix the diamine-terminated polysiloxane, 4-formylphenylboronic acid and DMF evenly, and stir for 3 hours at a rotation speed of 150 r / min and a temperature of 63°C to obtain intermediate 3. Mix the intermediate 3, anhydrous sodium sulfate and DMF evenly, and react at a temperature of 53°C under a nitrogen atmosphere for 25 hours to obtain a modified monomer.

[0046] The molar ratio of 2,6-diaminopyridine and 3-glycidyloxypropyldimethylmethoxysilane in step A1 is 1:2, the molar ratio of intermediate 1 and 4-vinylbenzoic acid is 1:2, and the amount of p-toluenesulfonic acid used is 1.3% of the mass of 4-vinylbenzoic acid.

[0047] The amount ratio of intermediate 2, diphenyldichlorosilane, deionized water and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane described in step A2 is 5 mmol:2 mmol:20 mL:5 mmol, and the amount of concentrated sulfuric acid is 2% of the mass of intermediate 1.

[0048] The molar ratio of the diamine-terminated polysiloxane to 4-formylphenylboronic acid in step A3 is 1:2, and the molar ratio of the intermediate 3 to anhydrous sodium sulfate is 1.3:4.2.

[0049] The flame retardant filler is prepared by the following steps:

[0050] Step B1: 2,2'-dihydroxybiphenyl and concentrated sulfuric acid are mixed, stirred at a speed of 120 r / min and a temperature of 23°C, and a nitric acid solution is added dropwise. After reacting for 4 hours, the mixture is cooled in an ice water bath, and the filtrate is removed by filtration to obtain an intermediate 4. Intermediate 4, tin and concentrated hydrochloric acid are mixed, and refluxed for 1.5 hours at a speed of 200 r / min and a temperature of 115°C. Concentrated ammonia water is added to adjust the pH value to 8, the mixture is boiled for 25 minutes, and the residue is removed by filtration. Glacial vinegar is added to the filtrate to adjust the pH value to 4, and the filtrate is removed by filtration to obtain a modifier;

[0051] Step B2: Evenly mix terephthalaldehyde, modifier and ethyl acetate, stir for 3 hours at a speed of 150 r / min and a temperature of 65°C, then add DOPO and methanol, cool to 23°C, and continue to react for 23 hours to obtain a treating agent, dissolve the treating agent in ethyl acetate, introduce nitrogen protection, stir and add ammonium polyphosphate at a speed of 150 r / min and a temperature of 25°C, heat to 68°C, react for 4.5 hours, heat to 85°C, keep warm and dry to obtain a flame retardant filler.

[0052] The amount ratio of 2,2'-dihydroxybiphenyl, concentrated sulfuric acid and nitric acid solution in step B1 is 0.02 mol:50 mL:15 mL, the mass fraction of concentrated sulfuric acid is 98%, the mass fraction of nitric acid solution is 50%, the amount ratio of intermediate 4, tin and concentrated hydrochloric acid is 3 g:8 g:20 mL, and the mass fraction of concentrated hydrochloric acid is 36%.

[0053] The molar ratio of terephthalaldehyde, modifier and DOPO in step B2 is 2:3:4, and the mass ratio of treating agent and ammonium polyphosphate is 3.5:5.

[0054] Example 3

[0055] A method for preparing a polystyrene composite material comprises the following steps:

[0056] The modified monomer, styrene and DMF were mixed evenly, stirred and azobisisobutyronitrile was added at a speed of 80 r / min and a temperature of 80°C, and reacted for 2 hours. Then, zinc nitrate hexahydrate and flame retardant filler were added, and the reaction was continued for 5 hours. The mixture was filtered and dried to obtain a polystyrene composite material.

[0057] The mass ratio of the modified monomer, propylene, zinc nitrate hexahydrate and flame retardant filler is 15:50:3:2, and the amount of azobisisobutyronitrile is 1% of the mass of the modified monomer.

[0058] The modified monomer is prepared by the following steps:

[0059] Step A1: 2,6-diaminopyridine, 3-glycidyloxypropyldimethylmethoxysilane and DMF were mixed evenly, and the mixture was reacted for 8 hours at a speed of 200 r / min, a temperature of 50° C. and a pH value of 11 to obtain intermediate 1; 4-vinylbenzoic acid, intermediate 1, p-toluenesulfonic acid and DMF were mixed evenly, and the mixture was reacted for 10 hours at a speed of 150 r / min and a temperature of 120° C. to obtain intermediate 2;

[0060] Step A2: Intermediate 2, diphenyldichlorosilane and deionized water were mixed, stirred for 15 min at a speed of 300 r / min and a temperature of 70° C., concentrated sulfuric acid and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane were added, and the reaction was carried out for 6 h. The pH was adjusted to neutral to obtain a diamine-terminated polysiloxane;

[0061] Step A3: Mix the diamine-terminated polysiloxane, 4-formylphenylboronic acid and DMF evenly, and stir for 3 hours at a speed of 200 r / min and a temperature of 65°C to obtain intermediate 3. Mix the intermediate 3, anhydrous sodium sulfate and DMF evenly, and react at a temperature of 55°C under a nitrogen atmosphere for 25 hours to obtain a modified monomer.

[0062] The molar ratio of 2,6-diaminopyridine and 3-glycidyloxypropyldimethylmethoxysilane in step A1 is 1:2, the molar ratio of intermediate 1 and 4-vinylbenzoic acid is 1:2, and the amount of p-toluenesulfonic acid used is 1.5% of the mass of 4-vinylbenzoic acid.

[0063] The amount ratio of intermediate 2, diphenyldichlorosilane, deionized water and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane described in step A2 is 5 mmol:2 mmol:20 mL:5 mmol, and the amount of concentrated sulfuric acid is 2% of the mass of intermediate 1.

[0064] The molar ratio of the diamine-terminated polysiloxane to 4-formylphenylboronic acid in step A3 is 1:2, and the molar ratio of the intermediate 3 to anhydrous sodium sulfate is 1.3:4.2.

[0065] The flame retardant filler is prepared by the following steps:

[0066] Step B1: 2,2'-dihydroxybiphenyl and concentrated sulfuric acid are mixed, stirred at a speed of 120 r / min and a temperature of 25°C, and a nitric acid solution is added dropwise. After reacting for 5 hours, the mixture is cooled in an ice water bath, and the filtrate is removed by filtration to obtain an intermediate 4. Intermediate 4, tin and concentrated hydrochloric acid are mixed, and refluxed for 1.5 hours at a speed of 200 r / min and a temperature of 120°C. Concentrated ammonia water is added to adjust the pH value to 8, the mixture is boiled for 30 minutes, and the residue is removed by filtration. Glacial vinegar is added to the filtrate to adjust the pH value to 4, and the filtrate is removed by filtration to obtain a modifier;

[0067] Step B2: Evenly mix terephthalaldehyde, modifier and ethyl acetate, stir for 3 hours at a speed of 200 r / min and a temperature of 65°C, then add DOPO and methanol, cool to 25°C, and continue to react for 25 hours to obtain a treating agent, dissolve the treating agent in ethyl acetate, introduce nitrogen protection, stir and add ammonium polyphosphate at a speed of 200 r / min and a temperature of 25°C, heat to 70°C, react for 5 hours, heat to 85°C, keep warm and dry to obtain a flame retardant filler.

[0068] The amount ratio of 2,2'-dihydroxybiphenyl, concentrated sulfuric acid and nitric acid solution in step B1 is 0.02 mol:50 mL:15 mL, the mass fraction of concentrated sulfuric acid is 98%, the mass fraction of nitric acid solution is 50%, the amount ratio of intermediate 4, tin and concentrated hydrochloric acid is 3 g:8 g:20 mL, and the mass fraction of concentrated hydrochloric acid is 36%.

[0069] The molar ratio of terephthalaldehyde, modifier and DOPO in step B2 is 3:4:6, and the mass ratio of treating agent and ammonium polyphosphate is 3.5:5.

[0070] Comparative Example 1

[0071] Compared with Example 1, this comparative example uses diamine-terminated polysiloxane instead of the modified monomer, and the remaining steps are the same.

[0072] Comparative Example 2

[0073] Compared with Example 1, this comparative example did not add intermediate 2, and the remaining steps were the same.

[0074] Comparative Example 3

[0075] Compared with Example 1, this comparative example uses ammonium polyphosphate instead of the flame retardant filler, and the other steps are the same.

[0076] The composite materials obtained in Examples 1-3 and Comparative Examples 1-3 were made into specimens with a length of 80 mm, a width of 10 mm and a thickness of 4 mm. The impact properties of the materials were tested in accordance with the standard of GB / T1043-93. The tensile strength of the specimens with a length of 80 mm, a width of 10 mm, a middle width of 4 mm and a thickness of 4 mm was tested in accordance with the standard of GB / T1040-92. The limiting oxygen index of the specimens with a length of 130 mm, a width of 6.5 mm and a thickness of 3 mm was tested in accordance with GB / T2406.2-2009. The vertical combustion test of the specimens with a length of 130 mm, a width of 13 mm and a thickness of 3 mm was performed in accordance with the standard of ASTM D3801. The test results are shown in the following table.

[0077]

[0078] It can be seen from the above table that the present invention has good mechanical properties and flame retardant effect.

[0079] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A method for preparing a polystyrene composite material, characterized in that: The specific steps include: The modified monomer, styrene and DMF are mixed and stirred, and azobisisobutyronitrile is added to react, and then zinc nitrate hexahydrate and flame retardant filler are added to continue the reaction, filter and dry to obtain a polystyrene composite material; The modified monomer is prepared by the following steps: Step A1: 2,6-diaminopyridine, 3-glycidyloxypropyldimethylmethoxysilane and DMF are mixed to react to obtain intermediate 1, and 4-vinylbenzoic acid, intermediate 1, p-toluenesulfonic acid and DMF are mixed to react to obtain intermediate 2; Step A2: After mixing and stirring the intermediate 2, diphenyldichlorosilane and deionized water, concentrated sulfuric acid and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane are added, and after reacting, the pH is adjusted to neutral to obtain a diamine-terminated polysiloxane; Step A3: mixing and stirring a diamine-terminated polysiloxane, 4-formylphenylboronic acid and DMF to obtain an intermediate 3, and mixing and reacting the intermediate 3, anhydrous sodium sulfate and DMF to obtain a modified monomer; The flame retardant filler is prepared by the following steps: Step B1: 2,2'-dihydroxybiphenyl and concentrated sulfuric acid are mixed and stirred, and a nitric acid solution is added dropwise. After reaction, the mixture is cooled in an ice water bath, and the filtrate is filtered to obtain an intermediate 4. After the intermediate 4, tin and concentrated hydrochloric acid are mixed and refluxed for reaction, concentrated ammonia water is added to adjust the pH value to 8, the water is boiled, and the filter residue is removed by filtering. Glacial vinegar is added to the filtrate to adjust the pH value to 4, and the filtrate is removed by filtering to obtain a modifier; Step B2: After mixing terephthalaldehyde, a modifier and ethyl acetate, DOPO and methanol are added, the temperature is lowered and the reaction is continued to obtain a treating agent, the treating agent is dissolved in ethyl acetate, nitrogen is introduced for protection, the mixture is stirred and ammonium polyphosphate is added, the temperature is raised for reaction, and a flame retardant filler is obtained.

2. The method for preparing a polystyrene composite material according to claim 1, characterized in that: The mass ratio of the modified monomer, styrene, zinc nitrate hexahydrate and flame retardant filler is 15:50:3:

2.

3. The method for preparing a polystyrene composite material according to claim 1, characterized in that: The molar ratio of 2,6-diaminopyridine and 3-glycidyloxypropyldimethylmethoxysilane in step A1 is 1:2, and the molar ratio of intermediate 1 and 4-vinylbenzoic acid is 1:

2.

4. The method for preparing a polystyrene composite material according to claim 1, characterized in that: The amount ratio of the intermediate 2, diphenyldichlorosilane, deionized water and 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane described in step A2 is 5mmol:2mmol:20mL:5mmol.

5. The method for preparing a polystyrene composite material according to claim 1, characterized in that: The molar ratio of the diamine-terminated polysiloxane to 4-formylphenylboronic acid in step A3 is 1:2, and the molar ratio of the intermediate 3 to anhydrous sodium sulfate is 1.3:4.

2.

6. The method for preparing a polystyrene composite material according to claim 1, characterized in that: The amount ratio of 2,2'-dihydroxybiphenyl, concentrated sulfuric acid and nitric acid solution in step B1 is 0.02mol:50mL:15mL, the mass fraction of concentrated sulfuric acid is 98%, the mass fraction of nitric acid solution is 50%, the amount ratio of intermediate 4, tin and concentrated hydrochloric acid is 3g:8g:20mL, and the mass fraction of concentrated hydrochloric acid is 36%.

7. The method for preparing a polystyrene composite material according to claim 1, characterized in that: The molar ratio of terephthalaldehyde, modifier and DOPO in step B2 is n:n+1:2n, where n is a natural number greater than 0, and the mass ratio of the treating agent to ammonium polyphosphate is 3.5:

5.

8. A polystyrene composite material, characterized in that: Prepared according to any one of claims 1 to 7.