Polyurethane composite material for lifting system frame and preparation method thereof

Through the treatment of modified glass fiber and carbon fiber, combined with isocyanate resin, a cross-linked network of high-energy chemical bonds is formed, which solves the problem of insufficient interface bonding performance of polyurethane composite materials in the existing technology and achieves higher mechanical properties and aging resistance. Providing an environmentally friendly alternative to elevator shaft frames.

CN118359787BActive Publication Date: 2024-10-18SHANGHAI CHUNXIN ELECTROMECHANICAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410789031.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-19
Publication Date
2024-10-18
Estimated Expiration
2044-06-19

AI Technical Summary

Technical Problem

Existing elevator shaft frames are mainly made of steel or aluminum alloy, which consumes a lot of energy during production and use. Moreover, polyurethane-carbon fiber composite materials have shortcomings in improving the interface bonding performance, especially the interface bonding strength between glass fiber and polyurethane. There is less research.

Method used

Modified glass fiber and carbon fiber are used through acid etching and electrochemical oxidation treatment to improve fiber surface activity and compatibility, combined with isocyanate resin to form a cross-linked network of high-energy chemical bonds, and enhance the mechanical properties and corrosion resistance of polyurethane composite materials.

Benefits of technology

The mechanical properties and aging resistance of polyurethane composite materials are significantly improved, making them suitable for lifting system frames, reducing dependence on aluminum alloys and reducing energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention provides a polyurethane composite material for a lifting system frame and a preparation method thereof, wherein the polyurethane composite material comprises a polyurethane resin, a modified glass fiber and a modified carbon fiber, and the modified glass fiber is treated with dilute acid to improve the surface activity of the glass fiber, and then the glass fiber after the dilute acid treatment is contacted with 5-hydroxytryptamine, and the surface of the glass fiber is covered with 5-hydroxytryptamine; the modified carbon fiber is prepared by reacting electrochemically treated carbon fiber with 2,3-epoxypropyl monoester itaconic acid. A chemical reaction can occur between the epoxy group on the surface of the obtained modified carbon fiber and the polyurethane matrix, and the obtained modified glass fiber and the modified carbon fiber can also form an intermolecular force with the polyurethane matrix, while improving the compatibility of the system, the tensile strength and aging resistance of the composite material are also increased.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of new environmentally friendly materials, and in particular to a polyurethane composite material for a lifting system frame and a preparation method thereof. Background Art

[0002] With the continuous improvement of people's living standards, the demand for home elevators in villas and self-built houses in rural areas is increasing. Compared with conventional passenger elevators, the main feature of home elevators is that they are for family use, with small load capacity (≤400kg) and low running speed (≤1.0m / s). Generally, there is no reserved elevator shaft in buildings, and the elevator needs to be equipped with a dedicated elevator frame for strength support and running channel.

[0003] The current elevator shaft frames are mainly steel frames or aluminum alloy frames, but the production of aluminum profiles and steel consumes huge energy, and the welding surface needs to be rust-proofed later. It can be seen that whether it is the production, transportation, or installation and maintenance links, huge amounts of electricity and energy are consumed, which runs counter to the concept of energy conservation and environmental protection.

[0004] Composite materials composed of polyurethane and glass fiber and / or carbon fiber are new environmentally friendly materials. They can change the structure of the energy industry and respond to the call for dual carbon goals, which is of far-reaching significance.

[0005] In terms of this application, polyurethane new materials have obvious advantages over aluminum alloy frames, which are mainly reflected in the following aspects: 1. Low density and light weight: The density of polyurethane composite materials is 2g / cm 3 , which is equivalent to 2 / 3 of the density of aluminum alloy; polyurethane composite material parts that achieve the same function are 15%~30% lighter than aluminum alloy parts, which brings convenience to subsequent transportation, installation and post-processing; 2. Excellent physical properties: polyurethane-glass fiber and / or carbon fiber composite materials have excellent physical properties. After testing, the longitudinal tensile strength and bending strength of the product can reach more than 1000MPa, while the traditional aluminum alloy frame takes 6063-T5 aluminum alloy as an example, its tensile strength and yield strength are 160MPa and 110MPa respectively. It can be seen that polyurethane-glass fiber and / or carbon fiber are more than 7 times higher in strength than aluminum alloy, with obvious advantages; 3. Corrosion resistance and aging resistance: polyurethane-glass fiber and / or carbon fiber composite materials have outstanding corrosion resistance, can resist corrosion from acids, alkalis and salts, and will not undergo hydrolysis reaction in humid air. They have excellent water resistance and aging resistance.

[0006] However, although polyurethane-carbon fiber composites have achieved some results in practical applications, they are subject to the inert environment of the carbon fiber surface. When they are composited with the matrix material, it is often necessary to modify the carbon fiber or glass fiber to improve the interface bonding performance of the composite material. Liu Jiawei et al. treated the carbon fiber surface by electrochemical oxidation combined with silane coupling agent, repairing the damage on the carbon fiber surface while bridging the carbon fiber and polyurethane through chemical reaction, thereby improving the interface bonding performance between carbon fiber and polyurethane (Liu Jiawei, Ye Hao, Liu Yinglong et al. Performance study of electrochemical oxidation / silane coupling agent treated carbon fiber surface reinforced polyurethane-based composites [J]. New Chemical Materials, 2024, Issue 3, 113-118, 123), but currently there are relatively few studies on improving the interface bonding strength between glass fiber and polyurethane. Summary of the invention

[0007] In order to enhance the interface bonding between carbon fiber and polyurethane-based materials and improve the mechanical properties, corrosion resistance and aging resistance of the obtained composite material, the present invention provides a polyurethane-glass fiber composite material for a lifting system frame and a preparation method thereof.

[0008] A polyurethane composite material for a lifting system frame comprises the following components by weight: 45-70 parts of polyether polyol, 67.5-130 parts of isocyanate, 2.2-10 parts of catalyst, 20-27 parts of functional additive, 20-38 parts of modified glass fiber and 35-55 parts of modified carbon fiber; wherein the modified glass fiber is prepared by etching the glass fiber with acid and treating it with 5-hydroxytryptamine; and the modified carbon fiber is prepared by electrochemically oxidizing the carbon fiber and treating it with 2,3-epoxypropyl monoester itaconic acid (CAS: 7748-43-8).

[0009] In some embodiments of the present invention, the preparation process of the modified glass fiber comprises the following steps:

[0010] S1: Heat the glass fiber at 300-400℃ to remove organic impurities on the surface. After the fiber cools down, soak it in an acid solution for 30-60min, wash it with water, and dry it.

[0011] S2: Immerse the glass fiber obtained in S1 in an organic solution containing 5-hydroxytryptamine, and heat it under reflux reaction for 3-6 hours under the catalysis of Lewis base to obtain the modified glass fiber.

[0012] Furthermore, the acid solution in S1 is 10-15% by mass of dilute hydrochloric acid, 50-60% by mass of dilute sulfuric acid, and 8.0-10.5% by mass of dilute phosphoric acid.

[0013] Furthermore, the mass ratio of the glass fiber to 5-hydroxytryptamine in S2 is 100-120:13-28.

[0014] In some embodiments of the present invention, the preparation process of the modified carbon fiber comprises the following steps:

[0015] SS1: Remove the organic impurities on the surface of the carbon fiber at 600-650℃ under the protection of inert gas, soak it in ketone solvent to remove the remaining soluble impurities, and dry it for use;

[0016] SS2: electrolyzing the carbon fiber treated with SS1 in an electrochemical device, deionizing, ultrasonicating and drying to obtain electrochemically oxidized carbon fiber;

[0017] SS3: The electrochemically oxidized carbon fiber obtained in SS2 is immersed in an organic solution containing 2,3-epoxypropyl monoester itaconic acid, heated under the action of a Lewis acid catalyst and kept at a constant temperature for 1-2 hours to obtain the modified carbon fiber.

[0018] Furthermore, the electrolysis conditions described in SS2 are: graphite rod as cathode, carbon fiber as anode, electrolyte as 5-12% bicarbonate solution by mass, electrolysis time 60-90s, current density 0.2-0.5A / m 2 .

[0019] Furthermore, the mass ratio of the electrochemically oxidized carbon fiber to 2,3-epoxypropyl monoester itaconic acid in SS3 is 73-95:12-20.

[0020] Furthermore, the quaternary ammonium salt catalyst in SS3 is at least one of N-methylpyridinium quaternary ammonium salt, N-propylpyridinium quaternary ammonium salt, and triethylammonium oxide; and the reaction temperature is 80-100°C.

[0021] The present invention also provides a method for preparing the above-mentioned polyurethane composite material for the lifting system frame, comprising the following steps: uniformly mixing the polyether polyol and the functional additive, then mixing with the isocyanate and preheating at 40-60°C for 3-5 minutes, then stirring at high speed for 2-3 minutes to obtain a polyurethane foaming liquid, pouring the liquid into a mold containing modified glass fiber and modified carbon fiber, curing in an oven for 1-2 hours, and finally cooling and demolding it at room temperature to obtain the polyurethane composite material.

[0022] Furthermore, the isocyanate is polymethylene phenyl polyisocyanate (MDI); and the functional additive is at least one of a flame retardant, a foam stabilizer, an antioxidant, an ultraviolet light absorber, and a foaming agent.

[0023] The preparation principle of the modified glass fiber used in the present invention is that the surface of the glass fiber is firstly subjected to acid etching treatment to improve its surface roughness, and the formed depressions and micropores are helpful to improve the interfacial bonding strength between the fiber and the polyurethane resin through the so-called "locking effect"; in addition, the acid etching can also generate hydroxyl groups on the fiber surface to form a large number of silanol groups, and then the hydroxyl groups of 5-hydroxytryptamine and the silanol groups undergo a dehydration condensation reaction to introduce the nitrogen-containing five-membered ring carrying the amino group into the glass fiber surface. The presence of the amino group and the nitrogen-containing five-membered ring greatly improves the compatibility and interfacial bonding strength between the modified glass fiber and the polyurethane.

[0024] The modification principle of the modified carbon fiber is to introduce oxygen-containing functional groups on the surface of the carbon fiber by electrochemical oxidation treatment to improve the surface activity of the carbon fiber, and then utilize the epoxy reaction activity of 2,3-epoxypropyl monoester itaconic acid to undergo a ring-opening addition reaction with the oxygen-containing functional groups (hydroxyl groups) on the surface of the carbon fiber to introduce ester groups and epoxy groups on the surface of the carbon fiber.

[0025] When preparing the polyurethane composite material, the silanol groups on the surface of the modified glass fiber will undergo ring-opening addition with the epoxy groups on the surface of the modified carbon fiber. In the system, the modified glass fiber and the modified carbon fiber react to form a cross-linked network containing high-energy chemical bonds around the polyurethane, thereby greatly improving the mechanical properties and tensile strength of the obtained polyurethane composite material.

[0026] Therefore, the inventors believe that when preparing the modified glass fiber, the mass ratio of the acid-etched glass fiber to 5-hydroxytryptamine should not exceed 100-120:13-28; so as to retain a portion of the silanol groups on the surface of the glass fiber. When preparing the modified carbon fiber, if too much 2,3-epoxypropyl monoester itaconic acid is introduced, it will affect the interface compatibility between the modified carbon fiber and the polyurethane. According to the test results, the mass ratio of the used 2,3-epoxypropyl monoester itaconic acid to the electrochemically oxidized carbon fiber should be 12-20:73-95, so as to obtain a polyurethane composite material with better performance.

[0027] Beneficial effects: Compared with the prior art, the present invention adds specially modified glass fiber and carbon fiber to polyurethane: on the one hand, the nitrogen-containing unsaturated five-membered ring with amino group introduced on the surface of the modified glass fiber and the oxygen-containing functional group on the surface of the modified carbon fiber are used to improve the interfacial bonding force between the modified glass fiber, the modified carbon fiber and the polyurethane; on the other hand, a ring-opening addition reaction occurs between the modified glass fiber and the modified carbon fiber to form a cross-linked network connected by high-energy chemical bonds around the polyurethane molecules. Ultimately, the mechanical properties of the polyurethane resin are effectively enhanced, its tensile strength and aging resistance are improved, and it is suitable for the lifting system frame. DETAILED DESCRIPTION

[0028] The present invention is further described in detail below in conjunction with the embodiments. It should be noted that the following embodiments and comparative examples are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various improvements within the concept of the present invention may be carried out without departing from the gist or scope of the present invention.

[0029] The following is an illustrative description of the preparation process of the modified glass fiber and modified carbon fiber used in the examples. The glass fiber used below was purchased from Chongqing International Composite Materials Co., Ltd., with a product number of ESC301C; the carbon fiber used was purchased from Shanghai Zhisheng Co., Ltd.

[0030] Modified glass fiber-1

[0031] S1: 100g of glass fiber was heated at 300℃ to remove organic impurities on the surface. After the fiber was cooled, it was immersed in a 12% dilute hydrochloric acid solution for 30min, washed with water, and dried. The acid-etched glass fiber weighed 95.6g.

[0032] S2: The glass fiber obtained in S1 is immersed in a xylene solution containing 12.428 g of 5-hydroxytryptamine, heated under reflux for reaction for 3 hours under the catalytic action of 2.16 g of aluminum chloride, and then filtered, washed and dried after cooling to room temperature to obtain the modified glass fiber-1.

[0033] Modified glass fiber-2

[0034] S1: 110g of glass fiber was heated at 350℃ to remove organic impurities on the surface. After the fiber was cooled, it was immersed in a 55% dilute sulfuric acid solution for 45min, washed with water, and dried. The acid-etched glass fiber weighed 106.5g.

[0035] S2: The glass fiber obtained in S1 is immersed in a xylene solution containing 19.364 g of 5-hydroxytryptamine, heated under reflux for 4 hours under the catalytic action of 3.78 g of tributylamine, and then filtered, washed and dried after cooling to room temperature to obtain the modified glass fiber-2.

[0036] Modified glass fiber-3

[0037] S1: 120g of glass fiber was heated at 400℃ to remove organic impurities on the surface. After the fiber was cooled, it was immersed in a 10.5% dilute nitric acid solution for 60min, washed with water, and dried. The acid-etched glass fiber weighed 115.9g.

[0038] S2: The glass fiber obtained in S1 is immersed in a xylene solution containing 27.05 g of 5-hydroxytryptamine, heated under reflux for 6 hours under the catalytic action of 7.15 g of ferric chloride, and then filtered, washed and dried after cooling to room temperature to obtain the modified glass fiber-3.

[0039] Modified glass fiber-4

[0040] The preparation process is the same as that of modified glass fiber-4, except that the mass of 5-hydroxytryptamine used is 33.8 g (the mass ratio of the acid-etched glass fiber to 5-hydroxytryptamine is 120:35).

[0041] Modified glass fiber-5

[0042] During the preparation, a sufficient amount of 5-hydroxytryptamine is used to completely replace the silanol groups on the surface of the glass fiber.

[0043] Modified carbon fiber-1

[0044] SS1: 146 g of carbon fiber was heated at 600 °C under nitrogen to remove surface organic impurities, and then soaked in acetone to remove remaining soluble impurities, and dried for later use;

[0045] SS2: The carbon fiber treated with SS1 was electrolyzed in an electrochemical device. The electrolysis conditions were as follows: graphite rod as cathode, carbon fiber as anode, electrolyte as 5% ammonium bicarbonate solution, electrolysis time of 60 s, and current density of 0.2 A / m 2 ; After deionization, ultrasonication and drying, electrochemically oxidized carbon fiber was obtained with a mass of 141.6 g;

[0046] SS3: The electrochemically oxidized carbon fiber obtained by SS2 was immersed in dichloromethane containing 23.28g of 2,3-epoxypropyl monoester itaconic acid, heated to 80°C under the action of 3.30g of dibutyltin dilaurate and kept at a constant temperature for 1h, cooled to room temperature, filtered, washed and dried to obtain the modified carbon fiber-1.

[0047] Modified carbon fiber-2

[0048] SS1: 170g carbon fiber was heated at 620°C under nitrogen to remove surface organic impurities, and then soaked in acetone to remove remaining soluble impurities, and then dried for later use;

[0049] SS2: The carbon fiber treated with SS1 was electrolyzed in an electrochemical device. The electrolysis conditions were as follows: graphite rod as cathode, carbon fiber as anode, 8% sodium bicarbonate solution as electrolyte, electrolysis time of 80 s, and current density of 0.3 A / m 2 ; After deionization, ultrasonication and drying, electrochemically oxidized carbon fiber was obtained with a mass of 168.5 g;

[0050] SS3: The electrochemically oxidized carbon fiber obtained by SS2 was immersed in dichloromethane containing 31.72g of 2,3-epoxypropyl monoester itaconic acid, heated to 90°C under the action of 8.01g of tetrabutyltin and kept at a constant temperature for 1h, cooled to room temperature, filtered, washed and dried to obtain the modified carbon fiber-2.

[0051] Modified carbon fiber-3

[0052] SS1: 190g carbon fiber was heated at 650°C under nitrogen to remove surface organic impurities, and then soaked in acetone to remove remaining soluble impurities, and then dried for later use;

[0053] SS2: The carbon fiber treated with SS1 was electrolyzed in an electrochemical device. The electrolysis conditions were as follows: graphite rod as cathode, carbon fiber as anode, electrolyte as 12% potassium bicarbonate solution, electrolysis time 90 s, current density 0.5 A / m 2 ; After deionization, ultrasonication and drying, electrochemically oxidized carbon fiber was obtained with a mass of 187.3g;

[0054] SS3: The electrochemically oxidized carbon fiber obtained from SS2 was immersed in dichloromethane containing 39.43g of 2,3-epoxypropyl monoester itaconic acid, heated to 100°C under the action of 11.34g of stannous octoate and kept at a constant temperature for 2h, cooled to room temperature, filtered, washed and dried to obtain the modified carbon fiber-3.

[0055] Modified carbon fiber-4

[0056] The preparation process is the same as that of modified carbon fiber-3, except that the mass of the 2,3-epoxypropyl monoester itaconic acid is 49.29 g (the mass ratio of the carbon fiber obtained by electrochemical treatment to the 2,3-epoxypropyl monoester itaconic acid is 95:25).

[0057] Example 1

[0058] 70g of polyether polyol (YD-889, hydroxyl value 405±10, purchased from Hebei Yadong Chemical Group Co., Ltd.) was evenly mixed with 3.5g of bis(dimethylaminoethyl) ether, 10g of flame retardant TCPP, 2.3g of foam stabilizer, and 21g of foaming agent, and then mixed with 105g of MDI and preheated at 40°C for 3min, and then stirred at high speed for 2min to obtain a polyurethane foaming liquid. The liquid was poured into a mold containing 38g of modified glass fiber-1 and 35g of modified carbon fiber-3, and cured in an oven for 1h. Finally, it was cooled and demolded at room temperature to obtain the polyurethane composite material.

[0059] Example 2

[0060] 45g of polyether polyol (YD-4110, hydroxyl value 460±15, purchased from Hebei Yadong Chemical Group Co., Ltd.) was evenly mixed with 5.4g of N-methylmorpholine, 10g of flame retardant TCPP, 2.3g of foam stabilizer, and 21g of foaming agent, and then mixed with 90g of MDI and preheated at 50°C for 4min, and then stirred at high speed for 2min to obtain a polyurethane foaming liquid. The liquid was poured into a mold containing 30g of modified glass fiber-2 and 45g of modified carbon fiber-1, and cured in an oven for 1h. Finally, it was cooled and demolded at room temperature to obtain the polyurethane composite material.

[0061] Example 3

[0062] 45g of polyether polyol (YD-204, hydroxyl value 460±15, purchased from Hebei Yadong Chemical Group Co., Ltd.) and 17.5g of polyether polyol (YD-380, hydroxyl value 380±10, purchased from Hebei Yadong Chemical Group Co., Ltd.) were mixed evenly with 3.05g of triethylene diamine, 10g of flame retardant TCPP, 2.3g of foam stabilizer, and 21g of foaming agent, and then mixed with 90g of MDI and preheated at 60°C for 5min, and then stirred at high speed for 3min to obtain a polyurethane foaming liquid, and the liquid was poured into a mold containing 20g of modified glass fiber-3 and 55g of modified carbon fiber-2, and cured in an oven for 2h. Finally, it was cooled and demolded at room temperature to obtain the polyurethane composite material.

[0063] Example 4

[0064] Same as Example 3, except that the modified glass fiber used is modified glass fiber-4.

[0065] Example 5

[0066] Same as Example 3, except that the modified glass fiber used is modified glass fiber-5.

[0067] Example 6

[0068] Same as Example 1, except that the modified carbon fiber used is modified carbon fiber-4.

[0069] Comparative Example 1

[0070] Same as Example 3, except that the mass of modified glass fiber-3 is 18 g.

[0071] Comparative Example 2

[0072] Same as Example 3, except that the modified glass fiber-3 is replaced by unmodified glass fiber.

[0073] Comparative Example 3

[0074] Same as Example 3, except that modified glass fiber-3 is not added.

[0075] Comparative Example 4

[0076] Same as Example 1, except that the mass of modified carbon fiber-3 is 30 g.

[0077] Comparative Example 5

[0078] Same as Example 1, except that the modified carbon fiber-3 is replaced by unmodified carbon fiber.

[0079] Comparative Example 6

[0080] Same as Example 1, except that modified carbon fiber-3 is not added.

[0081] Performance Testing:

[0082] Tensile strength: The tensile properties of glass fiber / nylon 6 composite materials were tested using an electronic universal tensile testing machine. The test standard was in accordance with GB / T 2567-2021, the tensile speed was 10 mm / min, and at least 5 specimens were tested for each sample and the average value was taken.

[0083] Notched impact strength: The notched impact strength of the test samples was tested on an electronic cantilever beam impact tester. Five samples were tested for each group of samples and the average value was taken.

[0084] Bending strength: Tested in accordance with GB / T 2567-2021;

[0085] Anti-aging: The polyurethane composite material is placed under a 45W medical ultraviolet lamp for continuous irradiation for 600 hours, and then taken out. If there is no aging, hardening and shrinkage, and the surface is not yellowed, the test result is judged as "qualified", otherwise it is "unqualified".

[0086] The test results are shown in Table 1:

[0087]

[0088] From the data in Table 1, it can be seen that the modification methods of the modified glass fiber and the modified carbon fiber used have a slight effect on the mechanical properties of the final polyurethane composite material, but do not affect the mechanical strength required when it is used as a lifting system frame. However, the amount of the modified glass fiber and modified carbon fiber used and whether they are modified or not have a negative impact on the mechanical properties and / or aging resistance of the polyurethane composite material that cannot be ignored, and it is expected to affect its safety when used as a lifting system frame.

[0089] In summary, the polyurethane composite material provided by the present invention has excellent tensile strength, notched impact strength and bending strength, and also has certain anti-aging properties. It can be used as a lifting system frame to replace aluminum alloy, reduce the cost of use, and has considerable application prospects.

Claims

1. A polyurethane composite material for a lifting system frame, characterized in that: The composition comprises the following components by weight: 45-70 parts of polyether polyol, 67.5-130 parts of isocyanate, 2.2-10 parts of catalyst, 20-27 parts of functional additive, 20-38 parts of modified glass fiber and 35-55 parts of modified carbon fiber; The modified glass fiber is prepared by acid etching and 5-hydroxytryptamine treatment of the glass fiber; the modified carbon fiber is prepared by electrochemical oxidation of the carbon fiber and 2,3-epoxypropyl monoester itaconic acid treatment; The preparation process of the modified glass fiber comprises the following steps: S1: Heat the glass fiber at 300-400℃ to remove organic impurities on the surface. After the fiber cools down, soak it in an acid solution for 30-60min, wash it with water, and dry it. S2: immersing the glass fiber obtained in S1 in an organic solution containing 5-hydroxytryptamine, heating and refluxing for 3-6 hours under the catalytic action of a Lewis base, thereby obtaining the modified glass fiber; the mass ratio of the glass fiber to the 5-hydroxytryptamine is 100-120:13-28; The preparation process of the modified carbon fiber comprises the following steps: SS1: Remove the organic impurities on the surface of the carbon fiber at 600-650℃ under the protection of inert gas, soak it in ketone solvent to remove the remaining soluble impurities, and dry it for use; SS2: electrolyzing the carbon fiber treated with SS1 in an electrochemical device, deionizing, ultrasonicating and drying to obtain electrochemically oxidized carbon fiber; SS3: The electrochemically oxidized carbon fiber obtained by SS2 is immersed in an inert organic solution containing 2,3-epoxypropyl monoester itaconic acid, heated under the action of a Lewis acid catalyst and maintained at a constant temperature for 1-2 hours to obtain the modified carbon fiber; the mass ratio of the electrochemically oxidized carbon fiber to 2,3-epoxypropyl monoester itaconic acid is 73-95:12-20.

2. The polyurethane composite material for a lifting system frame according to claim 1, characterized in that: The acid solution in S1 is 10-15% by mass of dilute hydrochloric acid, 50-60% by mass of dilute sulfuric acid, and 8.0-10.5% by mass of dilute phosphoric acid.

3. The polyurethane composite material for a lifting system frame according to claim 1, characterized in that: The electrolysis conditions described in SS2 are: graphite rod as cathode, carbon fiber as anode, electrolyte as 5-12% bicarbonate solution, electrolysis time 60-90s, current density 0.2-0.5A / m 2 .

4. The polyurethane composite material for a lifting system frame according to claim 1, characterized in that: The Lewis acid catalyst in SS3 is at least one of organic tin compounds; and the reaction temperature is 80-100°C.

5. The method for preparing the polyurethane composite material for the lifting system frame according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: uniformly mixing polyether polyol and functional additive, then mixing with isocyanate, preheating at 40-60°C for 3-5 minutes, and then stirring at high speed for 2-3 minutes to obtain polyurethane foaming liquid, pouring the liquid into a mold containing modified glass fiber and modified carbon fiber, curing in an oven for 1-2 hours, and finally cooling and demolding at room temperature to obtain the polyurethane composite material.

6. The method for preparing the polyurethane composite material for the lifting system frame according to claim 5, characterized in that: The isocyanate is polymethylene phenyl polyisocyanate; the functional additive is at least one of a flame retardant, a foam stabilizer, an antioxidant, an ultraviolet light absorber, and a foaming agent.

Citation Information

Patent Citations

  • Itaconic acid based water-base UV resin and preparation method thereof

    CN106750221A

  • Polymer biodegradable medical device

    US20060193892A1