A method and system for selecting and matching design parameters of AGM separators
By detecting the thickness uniformity, tensile strength and rebound difference of the AGM separator, combined with the wet pressure holding capability test, the problem of separator matching is solved, ensuring uniform internal pressure of the battery and improving the cycling performance and life of the battery.
Patent Information
- Application Number
- CN202410790559.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-06-19
AI Technical Summary
The prior art is difficult to match the optimal design parameters for different AGM partitions, resulting in large differences in internal pressure of the battery, affecting the cycle performance and life of the battery.
Through thickness uniformity detection, tensile strength detection, rebound difference detection, wet pressure holding capacity detection and extreme group pressure testing, combined with the assessment of the ultimate deviation rate, tensile strength reduction rate and rebound difference rate, suitable candidates are selected. and find the best dry compression rate through trial and error.
It realizes all-round inspection of AGM partitions, provides accurate data support, ensures uniform contact between the partitions and the positive and negative electrode plates of the battery, and improves the cycle performance and life of the battery.
Smart Images

Figure CN118364660B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method and a system for selecting and matching design parameters of an AGM separator, belonging to the technical field of lead-acid batteries. Background Art
[0002] AGM separator plays a very important role in VRLA battery: 1) Isolating positive and negative plates to prevent short circuit inside the battery; 2) Storing electrolyte to provide electrolyte for electrode reaction; 3) Providing channels for oxygen circulation, ion and water migration in the battery; 4) Ensuring internal assembly pressure of the battery and inhibiting expansion and shedding of active materials. Good AGM separator performance and suitable compression rate are the guarantee for ensuring battery group pressure and maintaining excellent battery cycle performance.
[0003] When battery manufacturers select AGM separators, the tests of the separators' tensile strength, resistance, maximum pore size, basis weight, elongation at break, wet pressure holding capacity, capillary acid absorption height, acid immersion weight loss, pressurized liquid absorption and other properties can all be carried out in accordance with GB / T 28535-2018 "Lead-acid Battery Separators". However, through battery performance testing and dissection of batteries, it is found that even if the separators of the same thickness are used in battery preparation, the differences between separators from different manufacturers are also large. The reason for this is that it is related to the fiber composition of the separator. For example, when designing the battery, the designer uses the separator of manufacturer A for measurement, while the separator of manufacturer B is used in actual production, the internal pressure of the battery may be quite different. In addition, the test method for wet pressure holding capacity in the national standard is: pressurize the separator to 40kPa for water injection test. This method can detect the wet pressure holding capacity of the AGM separator, but it is not universally adaptable to all AGM separators. In order to match the best parameters for different separators, targeted testing is required.
[0004] For example, Chinese patent publication number CN105628546A discloses a test method for detecting the performance of AGM partitions. A complete set of test methods for detecting the pressure changes of AGM partitions under different states and the acid absorption under the corresponding assembly pressure is designed. The peak pressure, stable pressure, saturated hydraulic absorption pressure, minimum hydraulic absorption pressure and acid absorption amount of the partition under the set pressure can be provided by a single test using a stretching machine, which provides a basis for the selection of partitions in actual production, but does not involve the problem of matching the best parameters for different partitions. Summary of the invention
[0005] The technical problem to be solved by the present invention is: to overcome the shortcomings of the prior art and provide a method and system for selecting and matching design parameters of AGM separators, which can fully detect the resilience of the separators, provide accurate data support for battery design, and match different separators to the best parameters.
[0006] The method for selecting and matching design parameters of an AGM partition described in the present invention includes partition selection and design parameter matching, wherein the partition is selected by assessing the limit deviation rate of thickness uniformity detection, the tensile strength reduction rate of tensile strength detection, and the rebound difference rate of rebound difference detection; the design parameter matching finds the optimal dry compression rate of the partition through wet pressure holding capacity detection, pole group pressure test, partition assembly pole group pressure reduction rate detection, and partition matching optimal dry compression rate.
[0007] Preferably, the partition selection comprises the following steps:
[0008] (1) Thickness uniformity test: randomly select several pieces of separator samples, determine the location of the test points, test the thickness of the separator under 10kPa, and calculate the limit deviation rate of all test points;
[0009] The limit deviation rate is used to evaluate the thickness uniformity of the separator. The pressure on different parts of the separator with good uniformity is more uniform, and the electrolyte on the contact surface of the plate and the separator is uniform. Therefore, the current distribution on the plate is uniform when the battery is discharged, which is beneficial to the battery capacity. At the same time, the separator is close to the plate to prevent the active material from falling off. The thickness of the separator with poor uniformity fluctuates greatly, which will cause a large deviation in the acid absorption of different parts of the separator, making the initial capacity of the battery at low rate discharge vary greatly. Therefore, the thickness uniformity is directly related to the consistency of the battery.
[0010] (2) Tensile strength test: stack several partition samples neatly and clamp them into the clamping plates of the pressure testing machine; test the thickness d0 of the partition under 10 kPa, adjust the distance between the two clamping plates to 0.75 d0, and keep it for 30 minutes; perform tensile strength tests on the compressed and uncompressed partitions, and calculate the tensile strength reduction rate;
[0011] The higher the tensile strength reduction rate is, the more likely it is that some of the fibers inside the separator have been damaged during the compression process, and that they may be more easily damaged during the battery charging and discharging process, thereby affecting their strength.
[0012] (3) Rebound difference test: stack several partition samples neatly and clamp them into the clamping plate of the pressure testing machine; pressurize to 10 kPa and hold for 30 seconds, measure and record the thickness d1 of the partition; pressurize to 20 kPa and hold for 30 seconds, measure and record the thickness d2 of the partition; pressurize from 10 kPa to 100 kPa in sequence and hold for 30 seconds, measure and record the thickness d3 to d4 of the partition. 10; After testing the thickness under 100 kPa, start unloading, first unload to 90 kPa and hold for 30 seconds, measure and record the thickness of the partition d9'; then unload to 80 kPa and hold for 30 seconds, measure and record the thickness of the partition d8'; unload from 10 kPa to 10 kPa and hold for 30 seconds, measure and record the thickness of the partition d1', and calculate the rebound difference rate;
[0013] The difference between the loading pressure and the unloading pressure is used to evaluate the resilience of the separator. The resilience performance can reflect the durability of the separator to a certain extent. The better the rebound ability of the separator, the better the durability. Batteries using separators with excellent resilience performance can maintain a higher pole group pressure during use, so that the separator has good contact performance with the positive and negative plates of the battery, which is conducive to the smooth exchange of electrolytes during the internal electrode reaction of the battery, thereby obtaining a good cycle life. Batteries using separators with poor resilience performance show lower assembly pressure when they fail. After the battery has been circulating for a period of time, the separator and the plate have poor contact, which is not conducive to the oxygen cycle, causing premature capacity loss of the positive plate and shedding of the positive active material, affecting the cycle life of the battery.
[0014] After the separators that have passed the national standard test are tested by three methods: limit deviation rate, tensile strength reduction rate and rebound difference rate, the influence of AGM separators on battery capacity and cycle life is further evaluated from the aspects of uniformity of contact between each part of the plate and electrolyte, the difficulty of fiber damage inside the separator, and the durability of the separator during battery cycling. The separators that have passed the assessment of limit deviation rate, tensile strength reduction rate and rebound difference rate are selected.
[0015] (4) Partition selection: The partitions are selected through the assessment of limit deviation rate, tensile strength reduction rate and rebound difference rate.
[0016] The thickness uniformity is evaluated by the limit deviation rate, the tensile strength is evaluated by the tensile strength reduction rate, and the resilience is evaluated by the difference rate between the loading pressure and the unloading pressure. The separators that have passed the national standard test and passed the limit deviation rate, tensile strength reduction rate and rebound difference rate assessment are selected.
[0017] Preferably, in step (1), the limit deviation rate δ 极限 :(D max -D min )×100 / D, unit: %; where D max is the maximum thickness, D min is the minimum thickness, D is the nominal thickness;
[0018] In step (2), the tensile strength reduction rate δ 拉伸 : (δ-δ 挤压)×100 / δ, unit: %; where δ is the tensile strength before extrusion, δ 挤压 is the tensile strength after extrusion;
[0019] In step (3), the rebound difference rate δ under n×10 kPa 回弹 :(d n -d n ')×100 / d1, unit: %.
[0020] Preferably, the step (4) is performed by limiting the deviation rate δ 极限 , tensile strength reduction rate δ 拉伸 and the rebound difference rate δ 回弹 The partitions that meet the selection value M≤0.0029 are the selected partitions.
[0021] Where M = δ 极限 ×δ 拉伸 ×δ 回弹 .
[0022] Preferably, the design parameter matching further comprises the following steps:
[0023] (5) Wet pressure holding capacity test: stack several baffle samples neatly together and put them into a sealed bag. Clamp the sealed bag in the clamping plate of the pressure testing machine. First test the thickness d under 10 kPa, then adjust the distance between the two clamping plates to 0.70d, 0.75d, 0.80d, and 0.85d, respectively, and keep them for 30 minutes, and record the pressure value P1; inject pure water into the sealed bag, and the pure water level should be parallel to the height of the baffle; let it stand for 1 hour, record the pressure value P2, and calculate the wet pressure reduction rate;
[0024] After the separator is wetted with water, the surface tension and friction coefficient of the wetted separator change, causing the separator to shrink and the pressure to decrease. The difference in the wet pressure reduction rate of different separators increases. Through the wet pressure holding capacity test, the pressure reduction rate of each separator after adding water at different compression rates can be determined. This can predict the internal pressure of the battery after acid filling, which is also a reference for determining the dry compression rate of the AGM separator.
[0025] (6) Electrode group pressure test: Take 2n separator samples, cut n positive plates and n+1 negative plates into the same size as the separators; use the battery assembly method to place two separators on both sides of each positive plate to assemble into n positive and n+1 negative electrode groups; first test the thickness D1 of the 2n separators and the thickness of each positive and negative electrode plate under 10kPa; calculate the thickness D of the electrode group when the separator is compressed to 0.70D1, 0.75D1, 0.80D1, and 0.85D1 respectively; put the electrode group into a sealed bag, clamp the sealed bag into the clamping plate of the pressure testing machine, adjust the distance between the two clamping plates to D and keep it for 30 minutes, and record the pressure value P3; inject sulfuric acid solution into the sealed bag, keep it for 1 hour, record the pressure value P4, and calculate the electrode group pressure reduction rate;
[0026] The wet pressure holding capacity test can roughly estimate the internal pressure of the battery after acid is added, but to obtain more accurate data it is necessary to simulate the actual production process, because the partition will be compressed to varying degrees during the battery assembly process.
[0027] (7) Separator assembly electrode group pressure reduction rate: Based on P1 of the wet pressure holding capacity test and P3 of the electrode group pressure test, calculate the separator pressure reduction rate during the electrode group assembly process;
[0028] Under the same compression rate, after being assembled into a pole group, the pressure will decrease to varying degrees, which is caused by the assembly process. The pressure of the assembled pole group is the closest to the actual production pressure, and the number of positive and negative raw plates in the pole group should be consistent with the actual production.
[0029] (8) Optimal dry compression ratio of partition matching: The optimal dry compression ratio m of AGM partition matching is calculated by trial and error method.
[0030] Preferably, the step (8) of matching the partition with the optimal dry compression rate specifically comprises the following steps:
[0031] (81) The best dry compression ratio for AGM separator matching is calculated by trial and error method. The pressure P4 in the extreme group pressure test is used as the reference data, and the internal pressure X0 of the designed battery after acid injection is used as the benchmark to calculate the pressure X.
[0032] (82) Taking the pressure P4 in the extreme group pressure test as the reference data, find the partition compression ratio m closest to X0, and find the P1 value and δ under this compression ratio. 极群 Value, combined with δ 装配 Calculate X to see if X is close to X0. If the difference is large, adjust the compression rate m and continue calculating until X is close to X0. At this time, m is the optimal dry compression rate of the partition.
[0033] Preferably, the wet pressure reduction rate δ in step (5) is 湿态: (P1-P2)×100 / P1, unit: %;
[0034] The rate of decrease of the pressure of the pole group in step (6) is δ 极群 : (P3-P4)×100 / P3, unit: %;
[0035] The diaphragm pressure reduction rate δ in step (7) 装配 : (P1-P3)×100 / P1, unit: %;
[0036] In step (81), the pressure X = P1×(1-δ 装配 )×(1-δ 极群 ), unit: kPa.
[0037] Preferably, the pure water in step (5) has a temperature of (25±2)°C.
[0038] Preferably, the sulfuric acid solution in step (6) is (1.280±0.005) g / ml (25° C.) sulfuric acid solution.
[0039] The system for selecting and matching design parameters of an AGM separator described in the present invention is applied to the method for selecting and matching design parameters of an AGM separator described above, and includes a limit deviation rate detection module, a tensile strength reduction rate detection module, a rebound difference rate detection module, a separator selection module, a wet pressure holding capacity test module, a pole group pressure test module, a separator assembly pole group pressure reduction rate module, and a separator matching optimal dry compression rate module;
[0040] Limit deviation rate detection module: used to calculate the limit deviation rate based on the limit deviation rate detection data;
[0041] Tensile strength reduction rate detection module: used to calculate the tensile strength reduction rate based on the tensile strength reduction rate detection data;
[0042] Rebound difference rate detection module: used to calculate the rebound difference rate based on the rebound difference rate detection data;
[0043] Partition selection module: used to calculate the selection value based on the data of limit deviation rate detection, tensile strength reduction rate detection, and rebound difference rate detection;
[0044] Wet pressure holding capacity test module: used to calculate the wet pressure reduction rate based on the data of the wet pressure holding capacity test;
[0045] Pole group pressure test module: used to calculate the pole group pressure reduction rate based on the pole group pressure test data;
[0046] Separator assembly pole group pressure reduction rate module: used to calculate the separator pressure reduction rate based on the data of wet pressure holding capacity test and pole group pressure test;
[0047] The module for optimal dry compression rate of partition matching is used to find the optimal dry compression rate based on the data of wet pressure holding capacity and extreme group pressure test.
[0048] The limit deviation rate detection module, tensile strength reduction rate detection module, rebound difference rate detection module, partition selection module, wet pressure holding capacity test module, pole group pressure test module, partition assembly pole group pressure reduction rate module and partition matching optimal dry compression rate module are used to calculate the data in the detection and testing process, improve the degree of automation, simplify the operation and speed up the calculation.
[0049] Compared with the prior art, the present invention has the following beneficial effects:
[0050] (1) In the present invention, thickness uniformity is evaluated by the limit deviation rate, tensile strength is evaluated by the tensile strength reduction rate, and resilience is evaluated by the difference rate between loading pressure and unloading pressure. The separators that have passed the national standard test and passed the assessment of the limit deviation rate, tensile strength reduction rate and resilience difference rate are selected.
[0051] (2) In the present invention, the compression rate of each separator under different pressures is determined through a rebound test, the thickness under unloading to 10 kPa is found, the rebound performance of the separator is evaluated, and the state of each separator during battery assembly and dry state is estimated, thereby providing data for battery design.
[0052] (3) In the present invention, the wet pressure holding capacity test is used to determine the pressure reduction rate of each separator after adding water at a certain compression rate, and the internal pressure of the battery after acid filling is predicted, which is also a reference for determining the dry compression rate of the AGM separator.
[0053] (4) In the present invention, through the pole group pressure test, it is clear that the pressure of the partition under pressure to a certain thickness is different from the pressure of the pole group under pressure to a certain thickness. To match the partition with a suitable compression rate, it is not enough to just test the partition. It is more reliable to assemble it into a pole group for simulation operation. After repeated tests, the best dry compression rate is finally matched for each AGM partition. BRIEF DESCRIPTION OF THE DRAWINGS
[0054] Figure 1 It is a schematic diagram of the location of the test points;
[0055] Figure 2 It is a structural schematic diagram of a pressure testing machine;
[0056] Figure 3 is the dry pressure variation curve of the partition;
[0057] Figure 4 This is the curve of acid injection pressure reduction rate.
[0058] Among them, 1. splint; 2. pressure display. DETAILED DESCRIPTION
[0059] In order to make the objectives, technical solutions and advantages of the present invention more clear, the embodiments of the present invention will be described in further detail below.
[0060] The present invention discloses a method for selecting and matching design parameters of AGM separators, using Figure 2 The pressure testing machine shown is used as the measuring instrument and the test is carried out as follows:
[0061] Thickness uniformity: Randomly select several pieces of partition samples with a size of 150mm×500mm. Figure 1 As shown in the figure, the positions of 7 test points are determined, and the thickness of the test diaphragm is tested under a pressure of 10 kPa (the pressure is obtained through the pressure display 2). The limit deviation rate δ of all points is calculated 极限 , δ 极限 ≤8% is the preferred standard.
[0062] Limit deviation rate δ 极限 :(D max -D min )×100 / D, unit: %.
[0063] D max : Maximum thickness; D min : minimum thickness; D: nominal thickness.
[0064] Tensile Strength Stack several 100mm×100mm partition samples neatly and clamp them into the clamping plate 1 of the pressure tester. Test the thickness d0 of the partition under 10kPa, adjust the distance between the two clamping plates 1 to 0.75d0, and keep it for 30 minutes. Perform tensile strength test on the partitions that have been squeezed and the partitions that have not been squeezed. Calculate the reduction rate of tensile strength δ 拉伸 , δ 拉伸 ≤18% is the preferred standard.
[0065] Tensile strength reduction rate δ 拉伸 : (δ-δ 挤压 )×100 / δ, unit: %.
[0066] δ: tensile strength before extrusion; δ 挤压 : Tensile strength after extrusion.
[0067] Rebound difference: stack several 100mm×100mm partition samples neatly and clamp them into the clamping plate 1 of the pressure tester. Pressurize to 10kPa and hold for 30s, measure and record the thickness d1 of the partition; pressurize to 20kPa and hold for 30s, measure and record the thickness d2 of the partition; continue to pressurize to 30kPa…100 kPa and hold for 30s, measure and record the thickness d 10 After testing the thickness at 100 kPa, start unloading, first unload to 90 kPa and hold for 30 seconds, measure and record the thickness of the partition d9'; then unload to 80 kPa and hold for 30 seconds, measure and record the thickness of the partition d8'; continue to unload to 70 kPa...10 kPa and hold for 30 seconds, measure and record the thickness of the partition d1'. Calculate the rebound difference rate δ 回弹 , δ 回弹 ≤20% (under 40kPa) is the preferred standard.
[0068] Rebound difference rate δ 回弹 : (d4-d4')×100 / d1, unit: %. (This formula calculates the rebound difference rate under 40kPa).
[0069] The selection of partitions passes the limit deviation rate δ 极限 , tensile strength reduction rate δ 拉伸 and rebound difference rate δ 回弹 The separators that meet the assessment of M≤0.0029 are selected. Where M=δ 极限 ×δ 拉伸 ×δ 回弹 , δ 回弹 The value is the rebound difference rate at 40 kPa. Subsequent tests were conducted to match the best dry compression rate.
[0070] Wet pressure holding capacity: Stack several 100mm×100mm partition samples neatly and put them into a sealed bag. Clamp the sealed bag in the clamp 1 of the pressure tester. First test the thickness d under 10kPa, then adjust the distance between the two clamps 1 to 0.70d, 0.75d, 0.80d, 0.85d, etc., keep it for 30 minutes, and record the pressure value P1. Inject pure water with a temperature of (25±2)℃ into the sealed bag. It is best if the liquid level of the pure water is parallel to the height of the partition. Let it stand for 1h and record the pressure value P2. Calculate the pressure reduction rate δ 湿态 . Draw a variation curve for P1.
[0071] Reduction rate δ 湿态 : (P1-P2)×100 / P1, unit: %.
[0072] Pole group pressure test Take several 100mm×100mm separator samples, cut n positive plates and n+1 negative plates into the same size as the separators. Measure the total thickness D1 of 2n separators at 10kPa, and the thickness of each positive and negative plate. Use the battery assembly method to place two separators on both sides of each positive plate to assemble into n positive and n+1 negative pole groups. First test the thickness D1 of 2n separators at 10kPa, and the thickness of each positive and negative plate. Calculate the thickness D of the pole group when the separator is compressed to 0.70D1, 0.75D1, 0.80D1, 0.85D1, etc. Put the pole group into a sealed bag, clamp the sealed bag into the clamping plate 1 of the pressure tester, adjust the distance between the two clamping plates 1 to D and keep it for 30 minutes, and record the pressure value P3. Inject (1.280±0.005)g / ml (25℃) sulfuric acid solution into the sealed bag, keep it for 1h, and record the pressure value P4. Calculate the pressure reduction rate δ 极群 , draw the curve of the pole group pressure reduction rate.
[0073] Reduction rate δ 极群 : (P3-P4)×100 / P3, unit: %.
[0074] The pressure reduction rate of the separator assembly electrode group is calculated based on P1 of the wet pressure holding capacity test and P3 of the electrode group pressure test. 装配 .
[0075] Reduction rate δ 装配 : (P1-P3)×100 / P1, unit: %.
[0076] The best dry compression rate for partition matching is calculated by trial and error method. The pressure P4 in the pole group pressure test is used as the reference data, and the pressure X is calculated based on the designed internal pressure X0 of the battery after acid injection.
[0077] X = P1×(1-δ 装配 )×(1-δ 极群 ), unit: kPa.
[0078] Take the pressure P4 in the extreme group pressure test as the reference data, find the partition compression ratio m closest to X0, find the P1 value and δ under this compression ratio 极群 Value, combined with δ 装配 Calculate X to see if X is close to X0. If the difference is large, adjust the compression rate m and continue calculating until X is close to X0. At this time, m is the optimal dry compression rate of the partition.
[0079] Example 1
[0080] This embodiment 1 discloses a method for selecting and matching design parameters of AGM separators, separators: separators from five manufacturers, A, B, C, D, and E, with a thickness of 2.15 mm (10 kPa). All five separators meet the requirements of GB / T 28535-2018 "Lead-acid Battery Separators".
[0081] Thickness uniformity: Randomly select 3 pieces of each type of separator from five manufacturers, A, B, C, D, and E, with a size of 150mm×500mm. Figure 1 As shown in the figure, the positions of 7 points are determined, the thickness of the separator is tested at 10kPa, and the limit deviation rate δ of 21 points of each separator is calculated 极限 , see Table 1.
[0082] Table 1 Limit deviation rate
[0083]
[0084] From the data in Table 1, it can be seen that the limit deviation rate δ of the A partition 极限 The highest, reaching 9.3%, does not meet the δ 极限 The preferred standard is ≤8%, and the other four separators meet the preferred standards.
[0085] Tensile strength Take the partitions of five manufacturers A, B, C, D, and E, cut them into samples with a size of 100mm×100mm, and clamp them into the clamping plate 1 of the pressure testing machine. Test the thickness d0 of the partition under 10kPa, adjust the distance between the two clamping plates 1 to 0.75d0, and keep it for 30min. Perform tensile strength test on the partitions that have been squeezed and the partitions that have not been squeezed. Calculate the tensile strength reduction rate δ 拉伸 , see Table 2.
[0086] Table 2 Tensile strength reduction rate
[0087]
[0088] From the data in Table 2, we can see that the tensile strength reduction rate δ of the separator of manufacturer A 拉伸 The highest, reaching 22.4%, does not meet the δ 拉伸 The preferred standard is ≤18%, and the other four separators meet the preferred standards.
[0089] Rebound Difference Take the separators of five manufacturers A, B, C, D, and E, cut them into samples with a size of 100mm×100mm, 10 pieces of each separator, stack them neatly, and clamp them into the clamping plate 1 of the pressure testing machine. Pressurize to 10kPa and hold for 30s, measure and record the thickness d1 of the separator; then pressurize to 20kPa and hold for 30s, measure and record the thickness d2 of the separator; continue to pressurize to 30kPa...100 kPa and hold for 30s, measure and record the thickness d 10After testing the thickness at 100 kPa, start unloading, first unload to 90 kPa and hold for 30 seconds, measure and record the thickness of the partition d9'; then unload to 80 kPa and hold for 30 seconds, measure and record the thickness of the partition d8'; continue to unload to 70 kPa...10 kPa and hold for 30 seconds, measure and record the thickness of the partition d1'. Calculate the partition rebound difference rate δ 回弹 , see Table 3.
[0090] Table 3 Rebound difference rate
[0091]
[0092] From the data in Table 3, it can be seen that the rebound difference rate δ of the A partition at 40 kPa 回弹 The highest, reaching 20.9%, does not meet the δ 拉伸 The preferred standard is ≤20%, and the other four separators meet the preferred standards.
[0093] Based on the test results of thickness uniformity, tensile strength and rebound difference, the A partition can be excluded. The M values of the four partitions B, C, D and E are 0.00007, 0.0018, 0.0005 and 0.001 respectively, which meet the selection criteria of M≤0.0029, and the subsequent test of matching the best dry compression rate will be carried out.
[0094] Wet pressure holding capacity Take the partitions of manufacturers B, C, D, and E, cut them into samples with a size of 100mm×100mm, 40 pieces of each kind of partition, 10 pieces in a group, stack them neatly together and put them into a sealed bag, clamp the sealed bag in the clamp 1 of the pressure testing machine, first test the thickness d under 10kPa, and then adjust the distance between the two clamps 1 to 0.70d, 0.75d, 0.80d, and 0.85d, that is, the compression rates are 30%, 25%, 20%, and 15%, respectively, keep for 30 minutes, and record the pressure value P1. Inject pure water with a temperature of (25±2)℃ into the sealed bag, and the pure water surface should be parallel to the height of the partition. Let it stand for 1h and record the pressure value P2. Calculate the pressure reduction rate δ 湿态 , see Table 4. Plot a curve of the dry pressure P1 of the partition in Table 4, see Figure 3 .
[0095] Table 4 Water injection pressure reduction rate
[0096]
[0097] From the data in Table 4, it can be seen that when the partition is compressed to a certain thickness and then water is injected, the pressure will decrease to varying degrees, and the reduction range is different. Taking 0.75d as an example, the reduction rate δ of the four partitions is 湿态 Between 27.3% and 31.5%.
[0098] The polar group pressure test takes the separators of four manufacturers, B, C, D, and E, and cuts them into samples with a size of 100mm×100mm, 80 pieces of each separator, 20 pieces in a group, and cuts 5 positive plates and 6 negative plates into the same size as the separator. Measure the total thickness D1 of the 20 separators at 10kPa, and the thickness of each positive and negative plate. Using the battery assembly method, put two separators on both sides of each positive plate to assemble into a polar group of 5 positive and 6 negative. First test the thickness D1 of the 20 separators at 10kPa, and the thickness of each positive and negative plate. Calculate the thickness D of the polar group when the separator is compressed to 0.70D1, 0.75D1, 0.80D1, and 0.85D1, that is, the compression rate is 30%, 25%, 20%, and 15%, respectively. Put the electrode group into a sealed bag, clamp the sealed bag into the clamping plate 1 of the pressure tester, adjust the distance between the two clamping plates 1 to D and keep it for 30 minutes, and record the pressure value P3. Inject (1.280±0.005)g / ml (25℃) sulfuric acid solution into the sealed bag, keep it for 1 hour, and record the pressure value P4. Calculate the pressure reduction rate δ 极群 , see Table 5. Pressure reduction rate δ 装配 The change curve of Figure 4 .
[0099] Table 5 Pressure reduction rate after acid injection
[0100]
[0101] After the acid is injected into the pole group, the pressure decreases to different degrees. Taking 0.75d1 as an example, the pressure reduction rate of the four types of partitions is δ 装配 In the range of 22.0% to 27.9%, the pressure reduction rate δ after water injection in the partition in the wet pressure holding capacity test is 湿态 (27.3%~31.5%) has decreased significantly.
[0102] 7. The pressure reduction rate of the partition assembly group
[0103] From the data comparison of P1 in Table 4 and P3 in Table 5, it can be seen that under the same compression rate, after being assembled into a pole group, the pressure of the partition will decrease to varying degrees, which is caused by the assembly process. When the partition is compressed to 0.75d1, that is, the compression rate is 25%, after being assembled into a pole group, the pressure reduction rate of the partition is δ 装配 , see Table 6.
[0104] Reduction rate δ 装配 : (P1- P3) × 100 / P1, unit: %.
[0105] Table 6 Assembled electrode group pressure reduction rate
[0106]
[0107] 8. The best dry compression ratio for the partition matching
[0108] The trial-and-error method is used to calculate the optimal dry compression rate of the AGM separator. Taking the pressure P4 in Table 5 as the reference data and the internal pressure of the battery after acid injection as 40 kPa, the dry compression rate of the separator is calculated.
[0109] From Table 5, we can see that the compression rate of B partition is between 20-25%. When it is closer to 25%, the pressure P4 is 40kPa. First calculate at 23%, from Figure 1 The curve shows that when the compression rate is 23%, the dry pressure of the partition is 65 kPa; from Table 6, the δ 装配 is 19.8%; Figure 2 It can be seen that when the compression rate is 23%, the δ of the B partition is 极群 is 23.5%; according to X = P1×(1-δ 装配 )×(1-δ 极群 ) is calculated, the X value is 39.9 kPa, so the best dry compression rate of B separator is 23%. The best dry compression rates of C, D, and E separators are calculated by this method, see Table 7.
[0110] Table 7 Optimum dry compression rate of partition
[0111]
[0112] Example 2
[0113] This embodiment 2 discloses a system for selecting and matching design parameters of AGM partitions, including a limit deviation rate detection module, a tensile strength reduction rate detection module, a rebound difference rate detection module, a partition selection module, a wet pressure holding capacity test module, a pole group pressure test module, a partition assembly pole group pressure reduction module and a partition matching optimal dry compression rate module.
[0114] Limit deviation rate detection module: used to calculate the limit deviation rate based on the limit deviation rate detection data;
[0115] Tensile strength reduction rate detection module: used to calculate the tensile strength reduction rate based on the tensile strength reduction rate detection data;
[0116] Rebound difference rate detection module: used to calculate the rebound difference rate based on the rebound difference rate detection data;
[0117] Partition selection module: used to calculate the selection value based on the data of limit deviation rate detection, the data of tensile strength reduction rate detection, and the data of rebound difference rate detection;
[0118] Wet pressure holding capacity test module: used to determine the pressure value and calculate the pressure reduction rate based on the data of the wet pressure holding capacity test;
[0119] Extreme group pressure test module: used to calculate the pressure reduction rate based on the data of extreme group pressure test;
[0120] Separator assembly pole group pressure reduction rate module: used to calculate the pressure reduction rate based on the data of wet pressure holding capacity test and pole group pressure test;
[0121] The module for optimal dry compression rate of partition matching is used to calculate the optimal dry compression rate based on the data of wet pressure holding capacity and extreme group pressure test.
[0122] The above embodiments are merely descriptions of preferred embodiments of the present invention and are not restrictive. Therefore, the present invention is not limited to the embodiments described in the specific embodiments. Any other embodiments derived by those skilled in the art based on the technical solutions of the present invention also fall within the scope of protection of the present invention.
Claims
1. A method for selecting and matching design parameters of AGM separators, characterized in that: Including partition selection and design parameter matching, partitions are selected through the assessment of the limit deviation rate of thickness uniformity test, the tensile strength reduction rate of tensile strength test and the rebound difference rate of rebound difference test; Design parameter matching is carried out through wet pressure holding capacity test, pole group pressure test, pole group pressure reduction rate test of the partition assembly and the best dry compression rate of the partition matching to find the best dry compression rate of the partition; The partition selection comprises the following steps: (1) Thickness uniformity test: randomly select several separator samples, determine the location of the test points, test the thickness of the separator under 10kPa, and calculate the limit deviation rate of all test points; (2) Tensile strength test: stack several partition samples neatly and clamp them into the clamping plates of the pressure testing machine; test the thickness d0 of the partition under 10 kPa, adjust the distance between the two clamping plates to 0.75 d0, and keep it for 30 minutes; perform tensile strength tests on the compressed and uncompressed partitions, and calculate the tensile strength reduction rate; (3) Rebound difference test: stack several partition samples neatly and clamp them into the clamping plate of the pressure testing machine; pressurize to 10 kPa and hold for 30 seconds, measure and record the thickness d1 of the partition; pressurize to 20 kPa and hold for 30 seconds, measure and record the thickness d2 of the partition; pressurize from 10 kPa to 100 kPa in sequence and hold for 30 seconds, measure and record the thickness d3 to d4 of the partition. 10 ; After testing the thickness under 100 kPa, start unloading, first unload to 90 kPa and hold for 30 seconds, measure and record the thickness of the partition d9'; then unload to 80 kPa and hold for 30 seconds, measure and record the thickness of the partition d8'; unload from 10 kPa to 10 kPa and hold for 30 seconds, measure and record the thickness of the partition d1', and calculate the rebound difference rate; (4) Selection of partitions: The partitions are selected through the assessment of limit deviation rate, tensile strength reduction rate and rebound difference rate; The design parameter matching also includes the following steps: (5) Wet pressure holding capacity test: stack several baffle samples neatly together and put them into a sealed bag. Clamp the sealed bag in the clamping plate of the pressure testing machine. First test the thickness d under 10 kPa, then adjust the distance between the two clamping plates to 0.70d, 0.75d, 0.80d, and 0.85d, respectively, and keep them for 30 minutes, and record the pressure value P1; inject pure water into the sealed bag, and the pure water level should be parallel to the height of the baffle; let it stand for 1 hour, record the pressure value P2, and calculate the wet pressure reduction rate; (6) Electrode group pressure test: Take 2n separator samples, cut n positive plates and n+1 negative plates into the same size as the separators; use the battery assembly method to place two separators on both sides of each positive plate to assemble into n positive and n+1 negative electrode groups; first test the thickness D1 of the 2n separators and the thickness of each positive and negative electrode plate under 10kPa; calculate the thickness D of the electrode group when the separator is compressed to 0.70D1, 0.75D1, 0.80D1, and 0.85D1 respectively; put the electrode group into a sealed bag, clamp the sealed bag into the clamping plate of the pressure testing machine, adjust the distance between the two clamping plates to D and keep it for 30 minutes, and record the pressure value P3; inject sulfuric acid solution into the sealed bag, keep it for 1 hour, record the pressure value P4, and calculate the electrode group pressure reduction rate; (7) Separator assembly electrode group pressure reduction rate: Based on P1 of the wet pressure holding capacity test and P3 of the electrode group pressure test, calculate the separator pressure reduction rate during the electrode group assembly process; (8) Optimal dry compression ratio of partition matching: The optimal dry compression ratio m of AGM partition matching is calculated by trial and error method.
2. A method for selecting and matching design parameters of AGM separators according to claim 1, characterized in that: In step (1), the limit deviation rate δ 极限 :(D max -D min )×100 / D, unit: %; where D max is the maximum thickness, D min is the minimum thickness, D is the nominal thickness; In step (2), the tensile strength reduction rate δ 拉伸 : (δ-δ 挤压 )×100 / δ, unit: %; where δ is the tensile strength before extrusion, δ 挤压 is the tensile strength after extrusion; In step (3), the rebound difference rate δ under n×10 kPa 回弹 :(d n -d n ')×100 / d1, unit: %.
3. A method for selecting and matching design parameters of AGM separators according to claim 2, characterized in that: The step (4) is performed by the limit deviation rate δ 极限 , tensile strength reduction rate δ 拉伸 and rebound difference rate δ 回弹 The separators that meet the selection value M≤0.0029 are selected as the selected separators; where M=δ 极限 ×δ 拉伸 ×δ 回弹 .
4. A method for selecting and matching design parameters of AGM separators according to claim 1, characterized in that: The step (8) of matching the partition with the optimal dry compression rate specifically comprises the following steps: (81) The best dry compression ratio for AGM separator matching is calculated by trial and error method. The pressure P4 in the extreme group pressure test is used as the reference data, and the internal pressure X0 of the designed battery after acid injection is used as the benchmark to calculate the pressure X. (82) Taking the pressure P4 in the pole group pressure test as the reference data, find the partition compression ratio m closest to X0, and find the P1 value and the pole group pressure reduction rate δ under this compression ratio. 极群 value, combined with the partition pressure reduction rate δ 装配 , calculate the pressure X, and see if X is close to X0. If the difference is large, adjust the compression rate m and continue calculating until X is close to X0. At this time, m is the optimal dry compression rate of the partition.
5. A method for selecting and matching design parameters of AGM separators according to claim 4, characterized in that: The wet pressure reduction rate δ in step (5) 湿态 : (P1-P2)×100 / P1, unit: %; The rate of decrease of the pressure of the pole group in step (6) is δ 极群 : (P3-P4)×100 / P3, unit: %; The diaphragm pressure reduction rate δ in step (7) 装配 : (P1-P3)×100 / P1, unit: %; In step (81), the pressure X = P1×(1-δ 装配 )×(1-δ 极群 ), unit: kPa.
6. A method for selecting and matching design parameters of AGM separators according to claim 1, characterized in that: The pure water in step (5) has a temperature of (25±2)°C.
7. A method for selecting and matching design parameters of AGM separators according to claim 1, characterized in that: The sulfuric acid solution in step (6) is (1.280±0.005) g / ml (25° C.) sulfuric acid solution.
8. A system for selecting and matching design parameters of AGM separators, applied to a method for selecting and matching design parameters of AGM separators as claimed in any one of claims 1 to 7, characterized in that: It includes limit deviation rate detection module, tensile strength reduction rate detection module, rebound difference rate detection module, partition selection module, wet pressure holding capacity test module, pole group pressure test module, partition assembly pole group pressure reduction rate module and partition matching optimal dry compression rate module; Limit deviation rate detection module: used to calculate the limit deviation rate based on the limit deviation rate detection data; Tensile strength reduction rate detection module: used to calculate the tensile strength reduction rate based on the tensile strength reduction rate detection data; Rebound difference rate detection module: used to calculate the rebound difference rate based on the rebound difference rate detection data; Partition selection module: used to calculate the selection value based on the data of limit deviation rate detection, tensile strength reduction rate detection, and rebound difference rate detection; Wet pressure holding capacity test module: used to calculate the wet pressure reduction rate based on the data of the wet pressure holding capacity test; Pole group pressure test module: used to calculate the pole group pressure reduction rate based on the pole group pressure test data; Separator assembly pole group pressure reduction rate module: used to calculate the separator pressure reduction rate based on the data of wet pressure holding capacity test and pole group pressure test; The module for optimal dry compression rate of partition matching is used to find the optimal dry compression rate based on the data of wet pressure holding capacity and extreme group pressure test.