High-strength and high-elongation MS adhesive and preparation method thereof

Through the combination of dendritic silane-modified resin and terminal double-bond polyether monool, combined with reinforcing fillers and plasticizers, the problems of complex process and low cross-linking degree of existing MS glue are solved, and high strength and high elongation are achieved. High-efficiency MS glue preparation simplifies the process and improves material performance.

CN118374263BActive Publication Date: 2024-10-15SHANDONG INOV NEW MATERIALS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410833669.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-15
Estimated Expiration
2044-06-26

AI Technical Summary

Technical Problem

The existing MS glue preparation process is complex, the material has a low degree of cross-linking, and the irritating substances used limit production, making it difficult to achieve high strength and high elongation properties.

Method used

Using dendritic silane modified resin and terminal double bond polyether monool through diisocyanate chain extension and silane coupling reaction, combined with reinforcing fillers and plasticizers, high strength and high elongation MS glue is prepared through simple process steps. Improved reactivity and mechanical properties.

Benefits of technology

MS glue that achieves high strength and high elongation simplifies the preparation process, reduces side reactions, improves the hardness and operability of the material, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention belongs to the field of adhesive technology, specifically relating to a high-strength, high-elongation MS adhesive and its preparation method. It is prepared by reacting component A and component B in a mass ratio of (12~15):1. Component A consists of the following raw materials in parts by weight: dendritic silane-modified resin: 29~35 parts; reinforcing filler: 40~83 parts; plasticizer I: 17~21 parts. Component B consists of the following raw materials in parts by weight: curing agent: 40~53 parts; plasticizer II: 37~42 parts; carbon black: 10~18 parts; catalyst: 0.25~0.4 parts. A chain extension reaction is carried out by adding diisocyanate to a terminal double-bond polyether monohydric alcohol with trimethylolpropane diallyl ether as an initiator, followed by an addition reaction with a silane coupling agent under the action of chloroplatinic acid catalyst to obtain the dendritic silane-modified resin. The resulting MS adhesive maintains its high elongation while also possessing high mechanical properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of adhesives, and in particular relates to high-strength and high-elongation MS adhesive and a preparation method thereof. Background Art

[0002] The most commonly used sealants on the market are polysulfide glue, silicone glue, and polyurethane glue. Polysulfide glue has a slow curing speed under low temperature conditions; silicone glue has poor water vapor penetration resistance and is not puncture-resistant; polyurethane glue has poor storage stability due to its terminal group -NCO. MS glue is a new sealant that has emerged in recent years. Its components do not contain any harmful solvents, and will not emit free formaldehyde and other substances that are harmful to humans. It is suitable for most building substrates; at the same time, because of its excellent construction performance, adhesion and paintability, it has a broad market background in the fields of building decoration, containers, and elevator industries.

[0003] CN110117357A introduces a silane-modified polyether and a preparation method thereof, wherein the preparation method is to prepare a siloxane-terminated modified polyether monomer of ethylene-linked silane by a silane-hydrogenation reaction of a vinyl resin and a hydrogen-containing silane, and the method requires the use of a vinyl-terminated agent to terminate the hydroxyl-terminated polyether, which is complex in process, has a low double bond content, and a low degree of crosslinking of the material. CN111704882A introduces a low modulus MS glue and a preparation method thereof, wherein the preparation method is to terminate a polyether polyol with a diisocyanate compound MDI first, and then terminate it with aniline methyl trimethoxy silane, primary amino silane, etc., to prepare an MS resin prepolymer, and the resin obtained by the method has a high viscosity, is prone to the risk of gelling polyreactor, and has poor operability. US Patent No. 9328272B2 introduces a silane-modified polyether, the preparation method of which is to first end-cap a polyether diol with allyl chloride to obtain a polyether with allyl end-capped at both ends, and then the allyl polyether is subjected to hydrosilylation with a trimethoxysilane monomer in the presence of chloroplatinic acid to obtain a trimethoxypropylsilane end-capped MS resin. This method requires the use of allyl chloride, a highly irritating substance, in production, and thus production is limited. In view of the current research status, it is of great significance to provide a MS glue with a simple preparation process and excellent performance. Summary of the invention

[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a high-strength and high-elongation MS glue. Through the carefully designed raw material molecular structure, the prepared MS glue has a unique dendritic main structure and a high terminal double bond content, so that the MS glue exhibits good reactivity and high cross-linking density, thereby giving it higher mechanical properties while maintaining its high elongation;

[0005] Another object of the present invention is to provide a method for preparing high-strength and high-elongation MS glue, which has a simple process, few side reactions, and is easy to mass produce.

[0006] The technical solution adopted by the present invention is as follows:

[0007] The high-strength and high-elongation MS adhesive is prepared by reacting component A and component B in a mass ratio of (12-15):1;

[0008] The A component is composed of the following raw materials in parts by weight:

[0009] Dendritic silane modified resin: 29-35 parts;

[0010] Reinforcing filler: 40~83 parts;

[0011] Plasticizer I: 17~21 parts;

[0012] The preparation steps of the dendritic silane modified resin are as follows: adding diisocyanate to a terminal double-bond polyether monool to carry out a chain extension reaction; after the chain extension reaction is completed, adding a silane coupling agent to carry out an addition reaction under the action of chloroplatinic acid catalyst to obtain the dendritic silane modified resin;

[0013] The terminal double-bond polyether monool uses trimethylolpropane diallyl ether as an initiator and has a number average molecular weight of 8500-18000;

[0014] The B component is composed of the following raw materials in parts by weight:

[0015] Curing agent: 40~53 parts;

[0016] Plasticizer II: 37~42 parts;

[0017] Carbon black: 10-18 parts;

[0018] Catalyst: 0.25~0.4 parts.

[0019] The preparation steps of the terminal double-bond polyether monool are as follows: trimethylolpropane diallyl ether is used as an initiator, under the action of a DMC catalyst, the temperature is raised to 130°C, 19-31wt.% of propylene oxide of the initiator is added dropwise to initiate, after the pressure drops to -0.08MPa, the remaining propylene oxide is catalyzed to undergo a ring-opening polymerization reaction, and after the reaction is completed, the monomer is removed for 0.5h to prepare the terminal double-bond polyether monool, and the amount of the DMC catalyst added is 30-71ppm of the terminal double-bond polyether monool.

[0020] The preparation steps of the dendritic silane modified resin are as follows: adding a terminal double-bond polyether monool into a reaction kettle, heating to 100-120°C, evacuating to -0.09-0.08MPa, dehydrating for 1.5-2h until the moisture content is less than 0.05wt.%, cooling to 60-80°C, adding diisocyanate for chain extension reaction, the chain extension reaction is carried out for 3-4h, after the -NCO content is 0, adding chloroplatinic acid catalyst and silane coupling agent for addition reaction, the addition reaction time is 3-4h, and the dendritic silane modified resin is obtained after the addition reaction is completed; the molar ratio of the terminal double-bond polyether monool, diisocyanate and silane coupling agent is (1.9-2.1):1:(3.9-4.2); the amount of the chloroplatinic acid catalyst added is 0.08-0.15wt.% of the total amount of the terminal double-bond polyether monool, diisocyanate and silane coupling agent.

[0021] The diisocyanate is one of toluene diisocyanate, diphenylmethane diisocyanate or hexamethylene diisocyanate; the silane coupling agent is one of trimethoxysilane, methyldimethoxysilane or triethoxysilane.

[0022] The reinforcing filler is one or more of white carbon black, nano calcium carbonate or heavy calcium carbonate.

[0023] The plasticizer I is one of dioctyl phthalate, diisononyl phthalate or dicyclohexyl phthalate.

[0024] The curing agent is one of polyamide resin, isophorone diamine or N,N-dimethylbenzylamine.

[0025] The plasticizer II is trifluoroethyl acrylate or trifluoroethyl methacrylate.

[0026] In the B component, the catalyst is one of dibutyltin dilaurate, dioctyltin dilaurate or stannous octoate.

[0027] The preparation method of the high-strength and high-elongation MS adhesive comprises the following steps:

[0028] S1: Add reinforcing filler and plasticizer I to the dendritic silane modified resin and stir for 0.5-1h to obtain component A;

[0029] S2: Add the curing agent and catalyst into the reaction kettle, raise the temperature to 90-100°C, evacuate to -0.09-0.08MPa and dehydrate for 1.5-2h until the moisture content is less than 0.05wt.%, cool down to 20-30°C, add plasticizer II and carbon black, stir evenly, and obtain component B;

[0030] S3: Mix component A and component B evenly and solidify to obtain high-strength and high-elongation MS adhesive.

[0031] Compared with the prior art, the present invention has the following beneficial effects:

[0032] (1) The dendritic silane modified resin of the present invention has a unique dendritic main structure and a high reactive group content, which can provide good reactivity and high crosslinking density for MS glue, thereby improving the strength and hardness of MS glue. At the same time, due to the long flexible chain segments contained in the structure, the MS glue can have a higher elongation;

[0033] (2) The dendritic silane modified resin described in the present invention is prepared by chain extension of a terminal double-bond polyether monool with a diisocyanate compound and then coupling reaction with a hydrogen-containing silane. The increase in the terminal double bond content increases the content of alkoxy groups participating in the reaction in the prepared dendritic silane modified resin, thereby obtaining excellent mechanical properties. This preparation method not only ensures a high terminal double bond content, but also the entire reaction process is carried out under mild conditions, and the operation steps are simple, easy to operate and easy to control;

[0034] (3) The present invention uses an alcohol compound containing an unsaturated double bond as an initiator, and catalyzes the ring-opening polymerization of propylene oxide under the action of a DMC catalyst to obtain a high molecular weight terminal double bond polyether monool. This preparation process is not only simple in process, but also has a high degree of terminal unsaturation of the product and significantly reduces side reactions. DETAILED DESCRIPTION

[0035] The present invention is further described below with reference to the embodiments, but they do not limit the implementation of the present invention.

[0036] The raw materials used in the examples and comparative examples are conventional commercially available raw materials unless otherwise specified, and the process methods used in the examples and comparative examples are conventional methods in the art unless otherwise specified.

[0037] Some of the raw materials used in the examples and comparative examples are described as follows:

[0038] INOVOL C2180 (with propylene glycol as the initiator and a number average molecular weight of 18,000) was purchased from Shandong INOVOL New Materials Co., Ltd.

[0039] Example 1

[0040] The preparation steps of the terminal double-bond polyether monool are as follows: 180g of trimethylolpropane diallyl ether and 0.22g of DMC catalyst are added into a high-pressure reactor, the temperature is raised to 130°C, 45g of propylene oxide is added dropwise to initiate, after the pressure drops to -0.08MPa, the remaining 6983g of propylene oxide is gradually added dropwise into the reactor, the pressure in the reactor is controlled to be ≤0.3MPa, and after the reaction is completed, the monomer is removed for 0.5h to prepare a terminal double-bond polyether monool with a functionality of 1, a hydroxyl value of 6.6mgKOH / g, and a number average molecular weight of 8500.

[0041] The preparation steps of the dendritic silane modified resin are as follows: 200g of terminal double-bond polyether monool is added into a reaction kettle, the temperature is raised to 110°C, the vacuum is evacuated to -0.09MPa for dehydration for 2h, the moisture content is tested to be 0.028wt.%, the temperature is lowered to 80°C, 2.05g of toluene diisocyanate is added for chain extension reaction, the chain extension reaction is carried out for 4h, after the -NCO content is tested to be 0, 0.2g of chloroplatinic acid catalyst and 7.72g of triethoxysilane are added for addition reaction, the addition reaction time is 3h, and the dendritic silane modified resin is obtained after the addition reaction is completed.

[0042] The preparation method of the high-strength and high-elongation MS adhesive comprises the following steps:

[0043] S1: Add 54.7 g of white carbon black, 273.6 g of nano calcium carbonate and 82.1 g of dioctyl phthalate to 136.8 g of dendritic silane modified resin and stir for 1 hour to obtain component A;

[0044] S2: Add 212g of polyamide resin and 1.4g of dibutyltin dilaurate into a reaction kettle, heat to 90°C, evacuate to -0.09MPa for dehydration for 2h, test the moisture content to be 0.02wt.%, cool to 25°C, add 148g of trifluoroethyl acrylate and 40g of carbon black, stir evenly, load, and seal with nitrogen to obtain component B;

[0045] S3: Mix component A and component B in a mass ratio of 12:1, stir thoroughly, and then cure to obtain high-strength and high-elongation MS glue.

[0046] Example 2

[0047] The preparation steps of the terminal double-bond polyether monool are as follows: 192g of trimethylolpropane diallyl ether and 0.55g of DMC catalyst are added into a high-pressure reactor, the temperature is raised to 130°C, 38g of propylene oxide is added dropwise to initiate, after the pressure drops to -0.08MPa, the remaining 10700g of propylene oxide is gradually added dropwise into the reactor, the pressure in the reactor is controlled to be ≤0.3MPa, and after the reaction is completed, the monomer is removed for 0.5h to prepare a terminal double-bond polyether monool with a functionality of 1, a hydroxyl value of 4.67mgKOH / g, and a number average molecular weight of 12013.

[0048] The preparation steps of the dendritic silane modified resin are as follows: 160g of terminal double-bond polyether monool is added into a reaction kettle, the temperature is raised to 100°C, the vacuum is evacuated to -0.09MPa for dehydration for 2h, the moisture content is tested to be 0.037wt.%, the temperature is lowered to 60°C, 1.66g of diphenylmethane diisocyanate is added for chain extension reaction, the chain extension reaction is carried out for 3h, after the -NCO content is tested to be 0, 0.22g of chloroplatinic acid catalyst and 2.83g of methyldimethoxysilane are added for addition reaction, the addition reaction time is 4h, and the dendritic silane modified resin is obtained after the addition reaction is completed.

[0049] The preparation method of the high-strength and high-elongation MS adhesive comprises the following steps:

[0050] S1: Add 66.4 g of nano calcium carbonate, 136.7 g of heavy calcium carbonate and 70.3 g of diisononyl phthalate to 117.2 g of dendritic silane modified resin, and stir for 0.5 h to obtain component A;

[0051] S2: 180g of isophoronediamine and 1g of dioctyltin dilaurate were added to a reaction kettle, the temperature was raised to 100°C, and the mixture was evacuated to -0.09MPa for dehydration for 1.5h. The moisture content was tested to be 0.026wt.%, and the temperature was lowered to 30°C. 160g of trifluoroethyl methacrylate and 60g of carbon black were added, the mixture was stirred evenly, loaded, and sealed with nitrogen to obtain component B;

[0052] S3: Mix component A and component B in a mass ratio of 13:1, stir thoroughly, and then cure to obtain high-strength and high-elongation MS glue.

[0053] Example 3

[0054] The preparation steps of the terminal double-bond polyether monool are as follows: 172g of trimethylolpropane diallyl ether and 1.04g of DMC catalyst are added into a high-pressure reactor, the temperature is raised to 130°C, 52g of propylene oxide is added dropwise to initiate, after the pressure drops to -0.08MPa, the remaining 14624g of propylene oxide is gradually added dropwise into the reactor, the pressure in the reactor is controlled to be ≤0.3MPa, and after the reaction is completed, the monomer is removed for 0.5h to prepare a terminal double-bond polyether monool with a functionality of 1, a hydroxyl value of 3.12mgKOH / g, and a number average molecular weight of 17981.

[0055] The preparation steps of the dendritic silane modified resin are as follows: 130g of terminal double-bond polyether monool is added into a reaction kettle, the temperature is raised to 120°C, the temperature is evacuated to -0.08MPa for dehydration for 1.5h, the moisture content is tested to be 0.031wt.%, the temperature is lowered to 70°C, 0.61g of hexamethylene diisocyanate is added for chain extension reaction, the chain extension reaction is carried out for 3h, after the -NCO content is tested to be 0, 0.11g of chloroplatinic acid catalyst and 1.86g of trimethoxysilane are added for addition reaction, the addition reaction time is 3h, and the dendritic silane modified resin is obtained after the addition reaction is completed.

[0056] The preparation method of the high-strength and high-elongation MS adhesive comprises the following steps:

[0057] S1: Add 54.1 g of white carbon black, 108.3 g of heavy calcium carbonate and 72.2 g of dicyclohexyl phthalate to 126.3 g of dendritic silane modified resin, and stir for 0.5 h to obtain component A;

[0058] S2: 160g N,N-dimethylbenzylamine and 1.6g stannous octoate were added to the reaction kettle, the temperature was raised to 100°C, and the vacuum was evacuated to -0.08MPa for dehydration for 1.5h. The moisture content was tested to be 0.026wt.%, and the temperature was lowered to 20°C. 168g trifluoroethyl acrylate and 72g carbon black were added, stirred evenly, loaded, and sealed with nitrogen to obtain component B;

[0059] S3: Mix component A and component B in a mass ratio of 15:1, stir thoroughly, and then cure to obtain high-strength and high-elongation MS glue.

[0060] Comparative Example 1

[0061] The preparation steps of the modified resin are as follows: adding 200g of INOVOL C2180 into a reactor, heating to 110°C, evacuating to -0.09MPa for dehydration for 2h, testing the moisture content to be 0.035wt.%, cooling to 80°C, adding 4.56g of isocyanatepropyltrimethoxysilane and 0.4g of dibutyltin dilaurate, and continuing the reaction for 3.5h to obtain a modified resin.

[0062] The preparation method of the high-strength and high-elongation MS adhesive comprises the following steps:

[0063] S1: Add 54.7 g of white carbon black, 273.6 g of nano calcium carbonate and 82.1 g of dioctyl phthalate to 136.8 g of modified resin and stir for 1 hour to obtain component A;

[0064] S2: Add 212g of polyamide resin and 1.4g of dibutyltin dilaurate into a reaction kettle, heat to 90°C, evacuate to -0.09MPa for dehydration for 2h, test the moisture content to be 0.023wt.%, cool to 25°C, add 148g of trifluoroethyl acrylate and 40g of carbon black, stir evenly, load, seal with nitrogen, and obtain component B;

[0065] S3: Mix component A and component B in a mass ratio of 12:1, stir well, and then cure to obtain MS glue.

[0066] Comparative Example 2

[0067] An allyl polyether with a number average molecular weight of 8500 is used to replace the synthetic modified resin of the terminal double-bond polyether monool in Example 1, wherein the allyl polyether is prepared by catalyzing the polymerization of propylene oxide under the action of DMC catalyst using allyl alcohol as an initiator, and the preparation steps are the same as the preparation steps of the terminal double-bond polyether monool described in Example 1.

[0068] The preparation steps of the modified resin are as follows: 200g of allyl polyether is added into a reaction kettle, the temperature is raised to 110°C, the vacuum is evacuated to -0.09MPa for dehydration for 2h, the moisture content is tested to be 0.024wt.%, the temperature is lowered to 80°C, 2.05g of toluene diisocyanate is added for chain extension reaction, the chain extension reaction is carried out for 4h, after the -NCO content is tested to be 0, 0.31g of chloroplatinic acid catalyst and 3.86g of triethoxysilane are added for addition reaction, the addition reaction time is 3h, and the modified resin is obtained after the addition reaction is completed.

[0069] The preparation method of the MS glue comprises the following steps:

[0070] S1: Add 54.7 g of white carbon black, 273.6 g of nano calcium carbonate and 82.1 g of dioctyl phthalate to 136.8 g of modified resin and stir for 1 hour to obtain component A;

[0071] S2: Add 212g of polyamide resin and 1.4g of dibutyltin dilaurate into a reaction kettle, heat to 90°C, evacuate to -0.09MPa for dehydration for 2h, test the moisture content to be 0.023wt.%, cool to 25°C, add 148g of trifluoroethyl acrylate and 40g of carbon black, stir evenly, load, seal with nitrogen, and obtain component B;

[0072] S3: Mix component A and component B in a mass ratio of 12:1, stir well, and then cure to obtain MS glue.

[0073] The performance tests were performed on the MS glues prepared in Examples 1 to 3 and Comparative Examples 1 to 2, respectively, and the test methods were as follows:

[0074] Refer to GB / T 531.1-2008 to test the molding hardness (Shore A);

[0075] Refer to GB / T 13477-2002 to test the surface drying time (min);

[0076] Refer to GB / T 528-2009, and test the tensile strength (MPa) and elongation at break (%) respectively;

[0077] Refer to GB / T 529-2008 to test the tear strength (N / mm);

[0078] The test results are shown in Table 1.

[0079] Table 1 Performance test results

[0080] project Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Molding hardness 54 51 48 39 41 Dry time 107 121 133 172 168 Tensile Strength 2.98 2.78 2.66 2.02 2.34 Tear Strength 5.62 4.97 4.60 4.38 4.80 Elongation at break 328 347 364 313 307

[0081] It can be seen from the test data in Table 1 that the MS glue prepared in Examples 1 to 3 can have a higher elongation due to the long flexible chain segments in the molecular structure; at the same time, due to the use of high unsaturation polyether polyols in the raw material components, the process is simple and the side reaction is low, which can greatly improve the crosslinking rate and degree of crosslinking, significantly improve the cohesion of the colloid, and thus improve the mechanical properties of the material. Compared with Example 1, the molecular weight of the modified resin in Comparative Example 1 is similar. Since Comparative Example 1 does not contain rigid segments except for the ends of the molecular structure, all of them are polyether segments, the mechanical properties after curing are poor; Compared with Example 1, Comparative Example 2 has a reduced double bond content, resulting in a reduced alkoxy content in the synthesized modified resin, which leads to a low crosslinking density, low hardness after curing, low reactivity, and a long curing time.

Claims

1. A high-strength and high-elongation MS adhesive, characterized in that: Prepared by reacting component A and component B in a mass ratio of (12~15):1; The A component is composed of the following raw materials in parts by weight: Dendritic silane modified resin: 29-35 parts; Reinforcing filler: 40~83 parts; Plasticizer I: 17~21 parts; The preparation steps of the dendritic silane modified resin are as follows: adding diisocyanate to a terminal double-bond polyether monool to carry out a chain extension reaction; after the chain extension reaction is completed, adding a silane coupling agent to carry out an addition reaction under the action of chloroplatinic acid catalyst to obtain the dendritic silane modified resin; The terminal double-bond polyether monool uses trimethylolpropane diallyl ether as an initiator and has a number average molecular weight of 8500-18000; The B component is composed of the following raw materials in parts by weight: Curing agent: 40~53 parts; Plasticizer II: 37~42 parts; Carbon black: 10-18 parts; Catalyst: 0.25~0.4 parts.

2. The high-strength and high-elongation MS adhesive according to claim 1, characterized in that: The preparation steps of the terminal double-bond polyether monool are as follows: trimethylolpropane diallyl ether is used as an initiator, and under the action of a DMC catalyst, propylene oxide is catalyzed to undergo a ring-opening polymerization reaction to prepare the monool.

3. The high-strength and high-elongation MS adhesive according to claim 1, characterized in that: The preparation steps of the dendritic silane modified resin are as follows: adding a terminal double-bond polyether monool into a reaction kettle, heating to 100-120°C, vacuum dehydrating to a moisture content of less than 0.05wt.%, cooling to 60-80°C, adding diisocyanate to carry out a chain extension reaction, after the chain extension reaction is carried out until the -NCO content is 0, adding a chloroplatinic acid catalyst and a silane coupling agent to carry out an addition reaction, the addition reaction time is 3-4h, and the dendritic silane modified resin is obtained after the addition reaction is completed; the molar ratio of the terminal double-bond polyether monool, the diisocyanate and the silane coupling agent is (1.9-2.1):1:(3.9-4.2); the amount of the chloroplatinic acid catalyst added is 0.08-0.15wt.% of the total amount of the terminal double-bond polyether monool, the diisocyanate and the silane coupling agent.

4. The high-strength and high-elongation MS adhesive according to claim 3, characterized in that: The diisocyanate is one of toluene diisocyanate, diphenylmethane diisocyanate or hexamethylene diisocyanate; the silane coupling agent is one of trimethoxysilane, methyldimethoxysilane or triethoxysilane.

5. The high-strength and high-elongation MS adhesive according to claim 1, characterized in that: The reinforcing filler is one or more of white carbon black, nano calcium carbonate or heavy calcium carbonate.

6. The high-strength and high-elongation MS adhesive according to claim 1, characterized in that: The plasticizer I is one of dioctyl phthalate, diisononyl phthalate or dicyclohexyl phthalate.

7. The high-strength and high-elongation MS adhesive according to claim 1, characterized in that: The curing agent is one of polyamide resin, isophorone diamine or N,N-dimethylbenzylamine.

8. The high-strength and high-elongation MS adhesive according to claim 1, characterized in that: The plasticizer II is trifluoroethyl acrylate or trifluoroethyl methacrylate.

9. The high-strength and high-elongation MS adhesive according to claim 1, characterized in that: In the B component, the catalyst is one of dibutyltin dilaurate, dioctyltin dilaurate or stannous octoate.

10. A method for preparing the high-strength and high-elongation MS adhesive according to any one of claims 1 to 9, characterized in that: Here are the steps: S1: Add reinforcing filler and plasticizer I to the dendritic silane modified resin and stir for 0.5-1h to obtain component A; S2: Add the curing agent and catalyst into the reaction kettle, raise the temperature to 90-100°C, vacuum dehydrate until the moisture content is less than 0.05wt.%, cool down to 20-30°C, add plasticizer II and carbon black, stir evenly, and obtain component B; S3: Mix component A and component B evenly and solidify to obtain high-strength and high-elongation MS adhesive.

Citation Information

Patent Citations

  • Silane modified polyether and preparation method thereof

    CN110117357A

  • Low-modulus MS adhesive and preparation method thereof

    CN111704882A

  • Curable composition

    US9328272B2

  • Modified silane polyether sealant and preparation method thereof

    CN109504333A

  • Composite two-component structural adhesive

    CN114437655A