Silicon carbide MOSFET power device and preparation method thereof
By utilizing the different oxidation rate characteristics of SiC materials in silicon carbide MOSFET power devices, a thickened gate dielectric layer is formed, which solves the problem of trench SiC MOSFET devices being easily damaged under high electric fields and improves the breakdown resistance and electrical performance. , suitable for high-performance mass production.
Patent Information
- Application Number
- CN202410814967.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-06-24
AI Technical Summary
The quality of the gate oxide layer of trench SiC MOSFET devices is difficult to control, which makes it easy to be damaged under high electric fields. Existing methods of thickening the gate dielectric will damage the electrical performance of the device or make it difficult to accurately control the thickness.
A silicon carbide MOSFET power device is designed. The first and second dielectric layers are formed at the bottom corners and side walls of the trench respectively. The different oxidation rates of each crystal face of the SiC material are used to form a thickened gate dielectric layer, and the gate dielectric layer is formed through high-temperature annealing. And the thermal oxidation process optimizes the thickness of the dielectric layer to ensure the structural integrity of the gate trench.
It significantly improves the anti-breakthrough capability of the device, reduces the risk of failure, and does not destroy the crystal structure of the SiC epitaxial layer. It achieves accurate control of the thickness of the gate dielectric, simplifies the process flow, and is suitable for high-performance mass production.
Smart Images

Figure CN118380475B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a power device and a manufacturing method thereof, in particular to a silicon carbide MOSFET power device and a manufacturing method thereof. Background Art
[0002] The development of power electronic systems has put forward higher requirements on the performance of semiconductor devices, especially in terms of high temperature, high frequency, radiation resistance, high voltage, etc. As a representative of the third generation of semiconductor materials, SiC has a larger bandgap, higher electron saturation drift velocity, stronger radiation resistance, higher breakdown electric field and thermal conductivity, which makes it have broad application prospects in power electronic equipment, aerospace systems, high-speed rail traction equipment, military electronic communication systems and other fields.
[0003] Compared with planar gate SiC MOSFET devices, trench SiC MOSFET devices form channels on the side walls of the trench, which not only improves the channel mobility but also eliminates the JFET effect, significantly reduces the on-resistance of the device, while reducing the cell size and increasing the power density.
[0004] However, the quality of the gate oxide layer of trench SiC MOSFET devices has always been a key factor limiting commercial production. Each crystal plane of SiC material has a different oxidation rate, which makes the gate oxide layer thickness of the trench sidewall 3 to 4 times that of the gate oxide layer at the bottom of the trench. In the off state, the curvature effect causes the thinner gate oxide layer at the bottom corner of the trench to withstand a higher electric field strength, causing destructive failure.
[0005] The gate dielectric material of SiC MOSFET devices that can be commercially produced at present is all SiO2. One of the ways to solve the problem of the gate dielectric being subjected to too high an electric field is to thicken the gate dielectric to improve the anti-breakdown capability of the SiO2 layer. The existing methods for thickening the gate dielectric layer include beating the SiC in the gate dielectric region into an amorphous state through heavy-dose ion implantation, using the higher oxidation rate of amorphous SiC to form a thickened gate dielectric, and depositing polysilicon at the bottom of the trench to form a thickened gate dielectric layer through a thermal oxidation process. However, the former will destroy the crystal structure of the SiC epitaxial layer near the gate dielectric and damage the electrical performance of the device; the latter cannot accurately control the thickness of the gate dielectric because it is difficult to control the oxidation rate of polysilicon. Summary of the invention
[0006] Purpose of the invention: In order to overcome the deficiencies in the prior art, the purpose of the present invention is to provide a silicon carbide MOSFET power device with significantly improved breakdown resistance and reduced failure risk. Another purpose of the present invention is to provide a simple and convenient method for preparing a silicon carbide MOSFET power device that can be mass-produced with high performance.
[0007] Technical solution: A silicon carbide MOSFET power device described in the present invention includes a drain electrode, and a substrate, an epitaxial layer, a well region, and a source region are sequentially arranged on the surface of the drain electrode; a gate trench is arranged on the epitaxial layer, the well region, and the source region, and the gate trench includes a first trench and a second trench, and the diameter of the first trench is greater than the diameter of the second trench, and a coaxial dielectric layer and a gate electrode are arranged in the gate trench; the dielectric layer includes a first dielectric layer arranged in the first trench and a second dielectric layer arranged in the second trench, and the thickness of the first dielectric layer is greater than the thickness of the second dielectric layer; an isolation dielectric layer is arranged on the surface of the gate electrode, the dielectric layer, and the source region, and a source electrode is also arranged on the surface of the source region.
[0008] Furthermore, the diameter of the first trench is 0.1 to 0.5 µm larger than the diameter of the second trench. This design can take advantage of the fact that each crystal plane of the SiC material has different oxidation rates, and form a thickened first dielectric layer at the bottom corner of the trench. The depth-to-width ratio of the first trench is ≤2:1, and the sidewall angle is ≥80 degrees. The depth-to-width ratio of the second trench is ≥1.5:1, and the sidewall angle is ≥80 degrees.
[0009] Furthermore, the distance between adjacent first grooves is not less than 1µm. The width of the first groove is 0.7-2µm, and the depth is 0.2-1.0µm; the width of the second groove is 0.5-1.8µm, and the depth is 0.5-2.0µm.
[0010] Furthermore, the dielectric layer further comprises a third dielectric layer, which is arranged at the center of the bottom of the gate trench and has a thickness of 40-150 nm. The dielectric layer is made of silicon dioxide material.
[0011] Furthermore, the substrate is made of 3C-SiC, 4H-SiC, 6H-SiC or 15R-SiC material, the thickness of the substrate is 10 ~1000µm, and the doping concentration is 1e18cm -3 ~5e19cm -3 , the doping elements are N, P and other elements.
[0012] Furthermore, the epitaxial layer is made of 3C-SiC, 4H-SiC, 6H-SiC or 15R-SiC material, the thickness of the epitaxial layer is 8 ~200µm, and the doping concentration is 1e14cm -3 ~1e16cm -3 .
[0013] Furthermore, the substrate, epitaxial layer, well region, and source region are all N-type or P-type.
[0014] Furthermore, the depth of the well region is 0.5 ~1.0µm, and the doping distribution of the well region can be uniform or non-uniform, with an average doping concentration of 5e16cm -3 ~5e17cm -3 .
[0015] Furthermore, the isolation dielectric layer is made of silicon nitride material with a thickness of 0.5-10µm to form a source window. Metal is evaporated through the source window, and the metal is selected from Ti / Al alloy, and then annealed at 300°C-1100°C to form a source ohmic contact. A drain ohmic contact is formed on the bottom layer of the substrate, a source electrode is formed on the surface of the source ohmic contact, and a drain electrode is formed on the surface of the drain ohmic contact layer.
[0016] A method for preparing a silicon carbide MOSFET power device according to the present invention comprises the following steps:
[0017] Step 1, growing an epitaxial layer, a well region, and a source region in sequence on a substrate;
[0018] Step 2: performing inductively coupled plasma etching on the epitaxial layer to remove part of the epitaxial layer and form a groove penetrating the well region and the source region;
[0019] Step 3, isotropically etching the bottom of the groove, and performing high temperature annealing and passivation at 1400° C. to 1800° C. to form a gate trench;
[0020] Step 4, forming a first dielectric layer at two bottom corners of the gate trench, forming a second dielectric layer at the sidewall of the gate trench, and performing high temperature annealing at 900° C. to 1300° C.;
[0021] Step five: forming a gate electrode in the dielectric layer, forming an isolation dielectric layer and a source electrode on the gate electrode and the surface of the source region, and forming a drain electrode on the substrate.
[0022] In order to further improve the anti-breakdown capability of the gate dielectric layer, step four is replaced by: forming a replacement layer in the bottom center of the gate trench, forming a first dielectric layer at the two bottom corners of the gate trench, forming a second dielectric layer at the sidewalls of the gate trench, annealing at a high temperature of 900°C to 1300°C, and thermally oxidizing the replacement layer to form a third dielectric layer.
[0023] Furthermore, in step one, the well region and the source region are formed by ion implantation, and the specific steps include: preparing a patterned mask layer on the surface of the epitaxial layer, then implanting first conductive type or second conductive type impurities, and annealing at 1400°C~2200°C for 2min~30min after removing the mask.
[0024] Furthermore, in step three, the gas used for high temperature annealing passivation is one or more of SiH4, H2, and Ar.
[0025] Furthermore, in step 4, the high temperature annealing gas is one or more of NO, N2O, H2, and NH3.
[0026] Furthermore, in step five, the gate electrode is polysilicon, amorphous silicon or amorphous silicon, and the doping impurities are Al, N, P or B. The gate electrode is formed by atomic layer deposition, chemical vapor deposition, plasma enhanced chemical vapor deposition or sputtering.
[0027] Working principle: In the off state, the thickened first dielectric layer has greatly enhanced its anti-breakdown capability, avoiding the risk of premature breakdown of the gate dielectric and causing the device breakdown voltage to fail to meet expectations, effectively improving device reliability.
[0028] Beneficial effects: Compared with the prior art, the present invention has the following significant features:
[0029] 1. It does not destroy the crystal structure of the SiC epitaxial layer, significantly improves the electrical performance of the device, and can accurately control the thickness of the gate dielectric;
[0030] 2. A gate trench is formed by connecting the first trench and the second trench, and a first dielectric layer at the bottom corner of the gate trench and a second dielectric layer at the sidewall of the second trench are formed by thermal oxidation. By utilizing the characteristic that each crystal plane of the SiC material has different oxidation rates, a thickened first dielectric layer is formed at the bottom corner of the trench, which significantly improves the anti-puncture capability of the bottom corner dielectric layer and greatly reduces the risk of device failure;
[0031] 3. The preparation method is compatible with the existing SiC trench-gate MOSFET power device manufacturing process, and only adds one isotropic etching process. Compared with the existing improved structure, the process complexity is significantly reduced, and it can be used to achieve high-performance trench-gate silicon carbide MOSFET device mass production. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 is a preparation flow chart of Example 1 of the present invention;
[0033] Figure 2 is a schematic structural diagram of a substrate 2 according to embodiment 1 of the present invention;
[0034] Figure 3 is a schematic structural diagram of the product obtained in step S1 of Example 1 of the present invention;
[0035] Figure 4 is a schematic structural diagram of the product obtained in step S2 of Example 1 of the present invention;
[0036] Figure 5 is a schematic diagram of the structure of the product obtained in step S3 of Example 1 of the present invention;
[0037] Figure 6 is a schematic diagram of the structure of the product obtained in step S4 of Example 1 of the present invention;
[0038] Figure 7is a schematic structural diagram of the product obtained in step S5 of Example 1 of the present invention;
[0039] Figure 8 is a schematic diagram of the structure of the product obtained in step S6 of Example 1 of the present invention;
[0040] Fig. 9 is a preparation flow chart of Example 2 of the present invention;
[0041] Fig.10 is a schematic structural diagram of a substrate 2 according to embodiment 2 of the present invention;
[0042] Fig.11 is a schematic diagram of the structure of the product obtained in step S1 of the present invention;
[0043] Fig.12 is a schematic structural diagram of the product obtained in step S2 of Example 2 of the present invention;
[0044] Fig.13 is a schematic structural diagram of the product obtained in step S3 of Example 2 of the present invention;
[0045] Fig.14 is a schematic structural diagram of the product obtained in step S4 of Example 2 of the present invention;
[0046] Fig.15 is a schematic structural diagram of the product obtained in step S5 of Example 2 of the present invention;
[0047] Fig.16 is a schematic structural diagram of the product obtained in step S6 of Example 2 of the present invention;
[0048] Fig.17 It is a schematic diagram of the structure of the product obtained in step S7 of Example 2 of the present invention. DETAILED DESCRIPTION
[0049] The experimental methods described in the examples are conventional methods unless otherwise specified; the reagents and materials are commercially available unless otherwise specified.
[0050] Example 1
[0051] like Figure 1 , a method for preparing a silicon carbide MOSFET power device, comprising the following steps:
[0052] S1, such as Figure 2~Figure 3 As shown, an epitaxial layer 3 is formed on the substrate 2 by epitaxial growth, and the thickness of the silicon carbide epitaxial layer 3 is 8µm~200µm, and the doping concentration is 1e14cm -3 ~1e16cm -3Substrate 2 is made of 3C-SiC, 4H-SiC, 6H-SiC or 15R-SiC material, with a thickness of 10 ~1000µm and a doping concentration of 1e18cm -3 ~5e19cm -3 , doping elements are N, P and other elements. The epitaxial layer is made of 3C-SiC, 4H-SiC, 6H-SiC or 15R-SiC materials. The thickness of epitaxial layer 3 is 8 ~200µm, and the doping concentration is 1e14cm -3 ~1e16cm -3 .
[0053] S2, such as Figure 4 As shown, an ion implantation mask layer is formed on the surface of the epitaxial layer 3 by a chemical vapor deposition process, and then a patterned etching mask layer is formed by a photolithography process. The patterned ion implantation mask layer is used to implant ions into the epitaxial layer 3 to form a well region 6. The depth of the well region 6 is 0.5µm~1.0µm, and the doping distribution can be uniform or non-uniform, with an average doping concentration of 5e16cm -3 ~5e17cm -3 After removing the mask, the source region 7 is formed in the same way. The depth of the source region 7 is 0.1µm~0.5µm and the doping concentration is 1e19cm -3 ~5e20cm -3 After the implantation is completed, the prepared device is annealed at 1400°C to 2200°C for 2min to 30min. The substrate 2, the epitaxial layer 3, the well region 6, and the source region 7 are all N-type or P-type.
[0054] S3, such as Figure 5 As shown, an etching mask layer is formed on the surface of the epitaxial layer 3 by chemical vapor deposition, and then a patterned etching mask layer is formed by photolithography. The epitaxial layer 3 is subjected to inductively coupled plasma etching using the patterned etching mask layer to remove part of the epitaxial layer 3, thereby forming a second trench 402 that penetrates the well region 6 and the source region 7, and then the etching mask layer is removed. The width of the second trench 402 is 0.5-1.8µm, and the depth is 0.5µm-2.0µm. The depth of the second trench 402 is greater than the depth of the well region 6, and the difference between the two is not less than 0.1µm.
[0055] S4, such as Figure 6As shown, an etching mask layer is formed on the surface of the epitaxial layer 3 and the sidewall and bottom of the second trench 402 by chemical vapor deposition, and then a patterned etching mask layer is formed by photolithography. The bottom of the second trench 402 is isotropically etched using the patterned etching mask layer to form a first trench 401 connected to the second trench 402. Subsequently, the etching mask layer is removed, and the trench is passivated by a high-temperature annealing process. The gas used can be one or more of SiH4, H2, Ar and the like. The annealing temperature is 1400°C to 1800°C. The first trench 401 and the second trench 402 form a gate trench 4. The width of the first trench 401 is 0.7µm to 2µm, and the depth is 0.2µm to 1.0µm. The width of the second trench 402 is 0.5 to 1.8µm, and the depth is 0.5 to 2.0µm. The width of the first trench 401 is greater than the width of the second trench 402, and the distance between adjacent first trenches 401 is not less than 1 μm. The sidewall angles of the first trench 401 and the second trench 402 are ≥80 degrees.
[0056] S5, such as Figure 7 As shown, a first dielectric layer 501 is formed at two bottom corners of the gate trench 4 by a thermal oxidation process, and a second dielectric layer 502 is formed at the sidewall of the second trench 402, and then a high-temperature annealing process is performed to improve the quality of the dielectric layer 5. The annealing gas may be one or more of NO, N2O, H2, NH3, etc., and the annealing temperature is 900° C. to 1300° C. The thickness of the first dielectric layer 501 is 70nm to 200nm, and the thickness of the second dielectric layer 502 is 40nm to 100nm.
[0057] S6, such as Figure 8 As shown, the gate electrode 8 is formed by chemical vapor deposition, photolithography and etching processes. The material of the gate electrode 8 is polysilicon. Polysilicon is injected and the polysilicon surface is flattened by CMP process. A patterned isolation dielectric layer 10 is formed by chemical vapor deposition, photolithography and etching processes. The material of the isolation dielectric layer 10 is silicon nitride with a thickness of 0.5-10µm to form a source window. Metal is evaporated through this source window. The metal is Ti / Al alloy, and then annealed at 300°C-1100°C to form a source ohmic contact. A drain ohmic contact is formed on the bottom layer of the substrate 2, a source electrode 9 is formed on the surface of the source ohmic contact, and a drain electrode 1 is formed on the surface of the drain ohmic contact layer.
[0058] The silicon carbide MOSFET power device obtained in this embodiment is composed of a drain electrode 1, a substrate 2, an epitaxial layer 3, a well region 6, and a source region 7 from bottom to top, and a gate trench 4 runs through the well region 6 and the source region 7 and extends into the epitaxial layer 3. The first trench 401 of the gate trench 4 contains a first dielectric layer 501, and the second trench 402 contains a second dielectric layer 502. A gate electrode 8 is provided in the hollow inside the dielectric layer 5. The upper surfaces of the gate electrode 8, the second dielectric layer 502, and the source region 7 are flush. An isolation dielectric layer 10 covers the surfaces of the gate electrode 8, the second dielectric layer 502, and part of the upper surface of the source region 7. There is also a source electrode 9 on the source region 7.
[0059] Example 2
[0060] like Fig. 9 , a method for preparing a silicon carbide MOSFET power device, comprising the following steps:
[0061] S1, such as Figure 10~Figure 11 As shown, an epitaxial layer 3 is formed on the substrate 2 by epitaxial growth, and the thickness of the silicon carbide epitaxial layer 3 is 8µm~200µm, and the doping concentration is 1e14cm -3 ~1e16cm -3 Substrate 2 is made of 3C-SiC, 4H-SiC, 6H-SiC or 15R-SiC material, with a thickness of 10 ~1000µm and a doping concentration of 1e18cm -3 ~5e19cm -3 , doping elements are N, P and other elements. The epitaxial layer is made of 3C-SiC, 4H-SiC, 6H-SiC or 15R-SiC materials. The thickness of epitaxial layer 3 is 8 ~200µm, and the doping concentration is 1e14cm -3 ~1e16cm -3 .
[0062] S2, such as Fig.12 As shown, Figure 4 As shown, an ion implantation mask layer is formed on the surface of the epitaxial layer 3 by a chemical vapor deposition process, and then a patterned etching mask layer is formed by a photolithography process. The patterned ion implantation mask layer is used to implant ions into the epitaxial layer 3 to form a well region 6. The depth of the well region 6 is 0.5µm~1.0µm, and the doping distribution can be uniform or non-uniform, with an average doping concentration of 5e16cm -3 ~5e17cm -3 After removing the mask, the source region 7 is formed in the same way. The depth of the source region 7 is 0.1µm~0.5µm and the doping concentration is 1e19cm -3 ~5e20cm -3After the implantation is completed, the prepared device is annealed at 1400°C to 2200°C for 2min to 30min. The substrate 2, the epitaxial layer 3, the well region 6, and the source region 7 are all N-type or P-type.
[0063] S3, such as Fig.13 As shown, an etching mask layer is formed on the surface of the epitaxial layer 3 by chemical vapor deposition, and then a patterned etching mask layer is formed by photolithography. The epitaxial layer 3 is subjected to inductively coupled plasma etching using the patterned etching mask layer to remove part of the epitaxial layer 3, thereby forming a second trench 402 that penetrates the well region 6 and the source region 7, and then the etching mask layer is removed. The width of the second trench 402 is 0.5-1.8µm, and the depth is 0.5µm-2.0µm. The depth of the second trench 402 is greater than the depth of the well region 6, and the difference between the two is not less than 0.1µm.
[0064] S4, such as Fig.14 As shown, an etching mask layer is formed on the surface of the epitaxial layer 3 and the sidewall and bottom of the second trench 402 by chemical vapor deposition, and then a patterned etching mask layer is formed by photolithography. The bottom of the second trench 402 is isotropically etched using the patterned etching mask layer to form a first trench 401 connected to the second trench 402. Subsequently, the etching mask layer is removed, and the trench is passivated by a high-temperature annealing process. The gas used can be one or more of SiH4, H2, Ar and the like. The annealing temperature is 1400°C to 1800°C. The first trench 401 and the second trench 402 form a gate trench 4. The width of the first trench 401 is 0.7µm to 2µm, and the depth is 0.2µm to 1.0µm. The width of the second trench 402 is 0.5 to 1.8µm, and the depth is 0.5 to 2.0µm. The width of the first trench 401 is greater than the width of the second trench 402, and the distance between adjacent first trenches 401 is not less than 1 μm. The sidewall angles of the first trench 401 and the second trench 402 are ≥80 degrees.
[0065] S5, such as Fig.15 As shown, a replacement layer 11 is formed at the bottom of the first trench 401 by chemical vapor deposition, photolithography and etching processes. The material of the replacement layer 11 can be polysilicon or amorphous silicon, and the thickness of the replacement layer 11 is 50nm~0.5µm.
[0066] S6, such as Fig.16As shown, a first dielectric layer 501 is formed at two bottom corners of the gate trench by a thermal oxidation process, a second dielectric layer 502 is formed at the sidewall of the second trench 402, and a third dielectric layer 503 is formed at the bottom of the first trench 401 away from the bottom corner, and then a high-temperature annealing process is performed to improve the quality of the dielectric layer 5. The annealing gas can be one or more of NO, N2O, H2, NH3, etc. The annealing temperature is 900°C to 1300°C. The thickness of the first dielectric layer 501 is 70nm to 200nm, the thickness of the second dielectric layer 502 is 40nm to 100nm, and the thickness of the third dielectric layer 503 is 40nm to 150nm. The third dielectric layer 503 is formed by thermal oxidation of the replacement layer 11, which can further improve the anti-breakthrough capability of the gate dielectric (dielectric layer 5).
[0067] S7, such as Fig.17 As shown, the gate electrode 8 is formed by chemical vapor deposition, photolithography and etching processes. The material of the gate electrode 8 is polysilicon. Polysilicon is injected and the polysilicon surface is flattened by CMP process. A patterned isolation dielectric layer 10 is formed by chemical vapor deposition, photolithography and etching processes. The material of the isolation dielectric layer 10 is silicon nitride with a thickness of 0.5~10µm to form a source window. Metal is evaporated through this source window. The metal is Ti / Al alloy, and then annealed at 300℃~1100℃ to form a source ohmic contact. A drain ohmic contact is formed on the bottom layer of the substrate 2, a source electrode 9 is formed on the surface of the source ohmic contact, and a drain electrode 1 is formed on the surface of the drain ohmic contact layer.
[0068] The silicon carbide MOSFET power device obtained in this embodiment has the same structure as the device obtained in Example 1, except that the dielectric layer 5 includes a first dielectric layer 501, a second dielectric layer 502, and a third dielectric layer 503. The third dielectric layer 503 is arranged at the center of the bottom of the gate trench 4 and has a thickness of 40-150 nm. The dielectric layer 5 is made of silicon dioxide material.
Claims
1. A method for preparing a silicon carbide MOSFET power device, characterized in that: The following steps are involved: Step 1: growing an epitaxial layer (3), a well region (6), and a source region (7) in sequence on a substrate (2); Step 2: performing inductively coupled plasma etching on the epitaxial layer (3) to remove part of the epitaxial layer (3) and form a groove that penetrates the well region (6) and the source region (7); Step 3, isotropically etching the bottom of the groove, and performing high temperature annealing and passivation at 1400° C. to 1800° C. to form a gate trench (4); Step 4, forming a replacement layer (11) at the bottom center of the gate trench (4), forming a first dielectric layer (501) at two bottom corners of the gate trench (4), forming a second dielectric layer (502) at the sidewalls of the gate trench (4), performing high temperature annealing at 900° C. to 1300° C., and thermally oxidizing the replacement layer (11) to form a third dielectric layer (503); Step 5: forming a gate electrode (8) in the dielectric layer (5), forming an isolation dielectric layer (10) and a source electrode (9) on the surface of the gate electrode (8) and the source region (7), and forming a drain electrode (1) on the substrate (2); The silicon carbide MOSFET power device comprises a drain electrode (1), wherein a substrate (2), an epitaxial layer (3), a well region (6), and a source region (7) are sequentially arranged on the surface of the drain electrode (1); a gate trench (4) is arranged on the epitaxial layer (3), the well region (6), and the source region (7), wherein the gate trench (4) comprises a first trench (401) and a second trench (402), wherein the diameter of the first trench (401) is greater than the diameter of the second trench (402), and wherein a coaxial dielectric layer (5) and a gate electrode (8) are arranged in the gate trench (4); wherein the dielectric layer (5) comprises a first dielectric layer (501) arranged in the first trench (401) and a second dielectric layer (502) arranged in the second trench (402), wherein the thickness of the first dielectric layer (501) is greater than the thickness of the second dielectric layer (502); an isolation dielectric layer (10) is arranged on the surfaces of the gate electrode (8), the dielectric layer (5), and the source region (7), and a source electrode (9) is also arranged on the surface of the source region (7); The thickness of the first dielectric layer (501) is 70 nm to 200 nm, and the thickness of the second dielectric layer (502) is 40 nm to 100 nm; the diameter of the first groove (401) is greater than the diameter of the second groove (402) by 0.1 to 0.5 µm; The dielectric layer (5) further comprises a third dielectric layer (503), wherein the third dielectric layer (503) is arranged at the center of the bottom of the gate trench (4) and has a thickness of 40-150 nm; The cross-sectional shape of the gate electrode (8) is T-shaped.
2. The method for preparing a silicon carbide MOSFET power device according to claim 1, characterized in that: The first groove (401) has a depth-to-width ratio of ≤2:1 and a sidewall angle of ≥80 degrees.
3. The method for preparing a silicon carbide MOSFET power device according to claim 1, characterized in that: The second trench (402) has a depth-to-width ratio of ≥1.5:1 and a sidewall angle of ≥80 degrees.
4. The method for preparing a silicon carbide MOSFET power device according to claim 1, characterized in that: The dielectric layer (5) is made of silicon dioxide material.
Citation Information
Patent Citations
Manufacturing method of shield gate trench MOSFET
CN112735953A
Trench-type power semiconductor device with low gate-drain charge and preparation method thereof
CN112864249A
Multistage groove type SiC MOSFET device and manufacturing method thereof
CN116154000A
Double-groove silicon carbide MOSFET device and manufacturing method thereof
CN117525154A