A composite solid electrolyte membrane and its preparation method and application
Through the composite solid electrolyte membrane structure and the superimposed heating and pressing technology of a variety of solid electrolyte materials, the problems of high interface impedance and poor mechanical properties in lithium-ion batteries are solved, and the safety performance and charge and discharge performance of the battery are improved.
Patent Information
- Application Number
- CN202410590991.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-13
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-05-13
Smart Images

Figure CN118380641B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of batteries, and in particular relates to a composite solid electrolyte membrane and a preparation method and application thereof. Background Art
[0002] Lithium-ion batteries are widely used due to their high energy density, good cycle stability, environmental friendliness, and wide operating temperature range. However, most lithium-ion batteries currently use flammable organic liquid electrolytes, which pose major safety hazards such as flatulence, leakage, fire, and explosion. Using non-flammable solid electrolytes to replace organic liquid electrolytes can fundamentally solve the safety problems of traditional liquid lithium-ion batteries. Therefore, the development of all-solid-state batteries with high safety, high energy density, and long cycle time has become a research focus.
[0003] At present, solid electrolytes are mainly divided into polymer electrolytes, oxide electrolytes, halide electrolytes and sulfide electrolytes. Among them, polymer electrolytes have good flexibility, easy film formation, simple preparation process, and good interface wettability with electrodes, but their room temperature ionic conductivity is low (<10 -5 S / cm), which seriously affects the performance of the battery; oxide electrolytes have high ionic conductivity (10 -4 ~10 -3 S / cm), with a wide electrochemical window, but its brittleness is large and the interface contact with the electrode is poor, which seriously limits its practical application; halide electrolytes have high ionic conductivity (10 -4 ~10 -3 S / cm) and a wide electrochemical window, but it is sensitive to moisture, easily degraded in air, and unstable to lithium metal; sulfide solid electrolytes have high ionic conductivity (10 -3 ~10 -2 S / cm) and become the solid electrolyte with the most application potential. However, sulfide solid electrolytes have a narrow electrochemical window, are unstable to lithium metal, and are sensitive to air and moisture, which limits their practical application.
[0004] Therefore, it is necessary to develop a solid electrolyte product that can improve the safety performance and charge and discharge performance of all-solid-state batteries. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a composite solid electrolyte membrane and a preparation method and application thereof, which can effectively improve the interface contact between the solid electrolyte and the positive and negative electrodes, reduce the interface impedance, and have good mechanical properties, thereby improving the safety performance and charge and discharge performance of the all-solid-state battery.
[0006] In a first aspect of the present invention, there is provided a composite solid electrolyte membrane, the composite solid electrolyte membrane comprising a first solid electrolyte membrane, a second solid electrolyte membrane and a third solid electrolyte membrane, wherein the second solid electrolyte membrane is located between the first solid electrolyte membrane and the third solid electrolyte membrane;
[0007] The raw materials for preparing the first solid electrolyte membrane include polymer A, lithium salt, a first solvent and a first solid electrolyte;
[0008] The raw materials for preparing the second solid electrolyte membrane include B polymer, a second solvent and a second solid electrolyte;
[0009] The raw materials for preparing the third solid electrolyte membrane include polysiloxane, A polymer and lithium salt;
[0010] The A polymer includes at least one of polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene (PVDF-HFP), polymethyl methacrylate (PMMA), polyethylene oxide (PEO) and polyacrylonitrile (PAN);
[0011] The first solid electrolyte comprises an oxide solid electrolyte;
[0012] The B polymer includes at least one of styrene-butadiene-styrene elastomer (SEBS), styrene-butadiene-styrene block copolymer (SBS), nitrile rubber (NBR), hydrogenated nitrile rubber (HNBR), butadiene rubber (BR), natural rubber (NR) and aliphatic polycarbonate (PPC);
[0013] The second solid electrolyte includes a sulfide solid electrolyte and / or a halide solid electrolyte.
[0014] In some embodiments of the present invention, the oxide solid electrolyte includes Li 1+a Al a Ti 2-a (PO4)3(LATP, 0≤a≤0.5), Li 1+b Al b Ge 2-b (PO4)3(LAGP, 0≤b≤0.65), La 2 / 3-c Li 3c TiO3(LLTO,0.04 <c<0.17)、La 0.56 Li 0.33+d Ti 1-d Al d O3(LLTAO, 0≤d≤0.06), Li7La3Zr2O 12 (LLZO), Li 6.4 Ln3Z 1.4Ta 0.6 O 12 (LLZTO) and Li 6.75 Ln3Z 1.75 Nb 0.25 O 12 At least one of (LLZONb).
[0015] In some embodiments of the present invention, the oxide solid electrolyte comprises (Li 1.3 Al 0.3 Ti 1.7 (PO4)3)(LATP), Li 1.5 Al 0.5 Ge 1.5 (PO4)3(LAGP), (La 0.56 Li 0.33 TiO3)(LLTO) and Li7La3Zr2O 12 At least one of (LLZO).
[0016] In some embodiments of the present invention, the second solid electrolyte includes Li6PS5Cl, Li6PS5Br, Li2S-P2S5, Li4GeS4, Li 10 GeP2S 12 , Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 、Li3PS4、Li7P3S 11 、Li3YCl6、Li3InCl6、Li 2-2x Mn 1+x Cl4(0≤x≤0.33), Li 2-2x Fe 1+x Cl4(0≤x≤0.33), Li 2-2x Mg 1+x Cl4(0≤x≤0.33), Li 2-2x Mn 1+x Br4(0≤x≤0.33) and Li 2-2x Mg 1+x At least one of Br4 (0≤x≤0.33).
[0017] In some embodiments of the present invention, the second solid electrolyte includes at least one of Li6PS5Cl, Li6PS5Br, Li3InCl6 and Li2S-P2S5.
[0018] In some embodiments of the present invention, the lithium salt includes at least one of LiTFSI, LiFSI, Li(CF3SO2)3C, LiC4F9SO3, LiN(SO2CF2CF3)2, LiB(C2O4)2, LiBF4, LiBF3(C2F5), LiSCN, LiN(CN)2, LiDFOB, LiODFB, LiN(SO2F)2, LiCF3SO3, LiClO4, LiAsF6 and LiSbF6.
[0019] In some embodiments of the present invention, the first solvent includes at least one of N-methylpyrrolidone (NMP), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), acetonitrile (ACN) and dimethyl sulfoxide (DMSO); and / or, the second solvent includes at least one of toluene, p-xylene, dichloromethane, dichloroethane, dichloropropane, dibromomethane, dibromoethane, dibromopropane, cyclohexane, n-heptane, n-decane, n-octane, anisole, butyl butyrate and benzyl acetate.
[0020] In some embodiments of the present invention, the thickness of the first solid electrolyte membrane is 1 to 10 μm, preferably 4 to 10 μm; and / or the thickness of the second solid electrolyte membrane is 15 to 40 μm, preferably 25 to 30 μm; and / or the thickness of the third solid electrolyte membrane is 1 to 10 μm, preferably 4 to 10 μm.
[0021] In some embodiments of the present invention, in the raw materials for preparing the first solid electrolyte membrane, the mass ratio of the lithium salt to the A polymer is (0.2-1):1, preferably (0.5-1):1; the mass ratio of the first solid electrolyte to the A polymer is (0.3-0.6):1.
[0022] In some embodiments of the present invention, in the raw materials for preparing the second solid electrolyte membrane, the mass ratio of the second solid electrolyte to the B polymer is (19-33):1, preferably (24-33):1.
[0023] In some embodiments of the present invention, in the raw materials for preparing the third solid electrolyte membrane, the mass ratio of the polysiloxane to the polymer A is (1-2):1, and the lithium salt accounts for 20-100wt.%, preferably 20-80wt.% of the total mass of the polysiloxane and the polymer A.
[0024] In a second aspect, the present invention provides a method for preparing the composite solid electrolyte membrane according to the first aspect of the present invention, comprising the following steps:
[0025] The first solid electrolyte membrane, the second solid electrolyte membrane and the third solid electrolyte membrane are stacked and then subjected to hot pressing to obtain a composite solid electrolyte membrane.
[0026] In some embodiments of the present invention, the temperature of the hot pressing is 80-150° C.; and / or the time of the hot pressing is 10-30 min; and / or the pressure of the hot pressing is 20-50 MPa.
[0027] In some embodiments of the present invention, the method for preparing the first solid electrolyte membrane comprises the following steps:
[0028] Mixing polymer A, lithium salt and a first solvent, and stirring at high speed at room temperature to obtain polymer A glue;
[0029] The first solid electrolyte and the first solvent are mixed, ultrasonically dispersed to form a uniform suspension, and mixed with the A polymer glue, and stirred at high speed at room temperature to obtain a first solid electrolyte slurry;
[0030] The first solid electrolyte slurry is coated on the base film and dried to obtain the first solid electrolyte membrane.
[0031] In some embodiments of the present invention, the method for preparing the second solid electrolyte membrane comprises the following steps:
[0032] Mixing the polymer B and the second solvent and stirring to obtain a polymer B glue solution;
[0033] The second solid electrolyte and the second solvent are mixed, ultrasonically dispersed to form a uniform suspension, and mixed and stirred with the B polymer glue to obtain a second solid electrolyte slurry;
[0034] The second solid electrolyte slurry is coated on the base film and dried to obtain the second solid electrolyte membrane.
[0035] In some embodiments of the present invention, the method for preparing the third solid electrolyte membrane comprises the following steps:
[0036] The polysiloxane, the A polymer and the lithium salt are mixed and stirred at high speed at room temperature to prepare a third solid electrolyte slurry;
[0037] The third solid electrolyte slurry is coated on the base film and dried to obtain a third solid electrolyte membrane.
[0038] In some embodiments of the present invention, the room temperature is 20-30°C.
[0039] In some embodiments of the present invention, the high-speed stirring is: stirring at a rate of 1000 to 2000 r / min for 30 to 60 min.
[0040] In some embodiments of the present invention, the ultrasonic dispersion time is 20 to 40 minutes.
[0041] In some embodiments of the present invention, the drying is: vacuum drying at 60-80° C. for 10-48 hours.
[0042] In some embodiments of the present invention, the base film includes a PET film, a copper foil or an aluminum foil.
[0043] According to a third aspect of the present invention, an all-solid-state battery is provided, comprising a positive electrode sheet, a negative electrode sheet and the composite solid electrolyte membrane according to the first aspect of the present invention.
[0044] In some embodiments of the present invention, the first solid electrolyte membrane is close to the positive electrode sheet, and the third solid electrolyte membrane is close to the negative electrode sheet.
[0045] In some embodiments of the present invention, the raw materials for preparing the positive electrode sheet include a positive electrode active material, a sulfide solid electrolyte, a conductive agent and a binder.
[0046] In some embodiments of the present invention, the mass ratio of the positive electrode active material, the sulfide solid electrolyte, the conductive agent and the binder is (70-90):(10-30):(1-3):(1.5-5).
[0047] In some embodiments of the present invention, the positive electrode active material includes at least one of lithium cobalt oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, lithium manganese oxide, lithium iron phosphate and lithium manganese iron phosphate.
[0048] In some embodiments of the present invention, the sulfide solid electrolyte includes Li6PS5Cl, Li6PS5Br, Li2S-P2S5, Li4GeS4, Li 10 GeP2S 12 , Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 , Li3PS4 and Li7P3S 11 At least one of .
[0049] In some embodiments of the present invention, the conductive agent includes at least one of Super P, CNTs, VGCF and acetylene black.
[0050] In some embodiments of the present invention, the binder includes at least one of SEBS, SBS, NBR, HNBR and BR.
[0051] In some embodiments of the present invention, the method for preparing the positive electrode sheet comprises the following steps:
[0052] The positive electrode active material, sulfide solid electrolyte, conductive agent and binder are added to the solvent and mixed thoroughly to prepare positive electrode slurry; the positive electrode slurry is evenly coated on aluminum foil, and the positive electrode sheet is obtained through conventional baking, rolling, striping and die-cutting processes.
[0053] In some embodiments of the present invention, the negative electrode sheet is a lithium metal electrode sheet.
[0054] In some embodiments of the present invention, the method for assembling the all-solid-state battery comprises the following steps:
[0055] The positive electrode sheet, the composite solid electrolyte membrane described in the first aspect of the present invention and the negative electrode sheet are assembled into an all-solid-state battery through conventional lamination, hot pressing and isostatic pressing processes.
[0056] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0057] 1. The composite solid electrolyte membrane provided by the present invention can effectively improve the interface contact between the solid electrolyte and the positive and negative electrodes and reduce the interface impedance by compounding two polymer-based solid electrolyte membranes (first and third solid electrolyte membranes) on the upper and lower sides of the second solid electrolyte membrane. At the same time, the polymer / oxide composite solid electrolyte (first solid electrolyte membrane) corresponding to the positive electrode side has strong oxidation resistance and can be applied to high-voltage positive electrode systems. The polysiloxane-based solid electrolyte membrane (third solid electrolyte membrane) corresponding to the negative electrode side has a high affinity for metallic lithium and can capture lithium ions on the surface and uniformly regulate the lithium ion flux, thereby achieving dendrite-free lithium deposition / stripping. In addition, the polysiloxane-based solid electrolyte membrane can play a protective role to prevent the lithium metal negative electrode from directly contacting the sulfide / halide solid electrolyte in the second solid electrolyte membrane, which causes serious side reactions.
[0058] 2. The composite solid electrolyte membrane provided by the present invention, the second solid electrolyte membrane in the middle layer contains a sulfide solid electrolyte and / or a halide solid electrolyte, which can improve the lithium ion conductivity and density of the solid electrolyte membrane, thereby inhibiting the growth of lithium dendrites. In combination with the flexible polymer-based solid electrolyte membranes (first and third solid electrolyte membranes) on the upper and lower sides, the flexibility of the composite solid electrolyte membrane can be increased, thereby improving the tensile strength. The composite solid electrolyte membrane thus obtained exhibits the advantages of high strength, good flexibility, good thermal stability and high ion conductivity, thereby improving the safety performance and charge and discharge cycle performance of the solid-state battery;
[0059] 3. The preparation method of the composite solid electrolyte membrane provided by the present invention has a simple process, is compatible with traditional lithium-ion battery process equipment, and is conducive to large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0060] Figure 1 is a schematic structural diagram of the composite solid electrolyte membrane of the present invention;
[0061] Figure 2 It is a schematic structural diagram of the all-solid-state battery of the present invention.
[0062] The markings in the accompanying drawings are as follows: 100, first solid electrolyte membrane; 200, second solid electrolyte membrane; 300, third solid electrolyte membrane; 400, positive electrode sheet; 500, negative electrode sheet. DETAILED DESCRIPTION
[0063] The present invention is further described in detail below by specific examples. The raw materials, reagents or devices used in the examples can be obtained from conventional commercial sources or by prior art methods unless otherwise specified. Unless otherwise specified, the experiments or test methods are conventional methods in the art.
[0064] In the description of the present invention, it should be understood that descriptions involving orientation, such as orientation or positional relationship indicated as up, down, etc., are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.
[0065] In the description of the present invention, if there is a description of first, second, and third, it is only for the purpose of distinguishing technical features, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features or implicitly indicating the sequence of the indicated technical features.
[0066] Example 1
[0067] like Figure 1 As shown, a composite solid electrolyte membrane includes a first solid electrolyte membrane 100 , a second solid electrolyte membrane 200 and a third solid electrolyte membrane 300 , wherein the second solid electrolyte membrane 200 is located between the first solid electrolyte membrane 100 and the third solid electrolyte membrane 300 .
[0068] The specific preparation method of the above composite solid electrolyte membrane is as follows:
[0069] 1. PVDF-HFP, LiTFSI and NMP were mixed and stirred at high speed at room temperature to prepare a clear and transparent PVDF-HFP glue solution; wherein the stirring rate was 1000 r / min, the stirring time was 30 min, and the mass ratio of PVDF-HFP to LiTFSI was 1:0.5;
[0070] 2. LATP (Li 1.3 Al 0.3 Ti 1.7 (PO4)3) and NMP were mixed, ultrasonically dispersed for 30 minutes to form a uniform suspension, and mixed with PVDF-HFP glue, and stirred at high speed at room temperature to obtain a first solid electrolyte slurry; wherein the stirring rate was 1200r / min, the stirring time was 30min, and the mass ratio of LATP to PVDF-HFP was 0.4:1;
[0071] 3. The first solid electrolyte slurry was coated on a PET film and vacuum dried at 60° C. for 24 h to obtain a first solid electrolyte membrane with a thickness of 5 μm;
[0072] 4. Mix and stir SEBS and p-xylene to prepare a clear and transparent SEBS glue;
[0073] 5. Li6PS5Cl and p-xylene were mixed, ultrasonically dispersed for 30 minutes to form a uniform suspension, and mixed with SEBS glue, and stirred thoroughly to obtain a second solid electrolyte slurry; wherein the mass ratio of Li6PS5Cl to SEBS was 33:1;
[0074] 6. The second solid electrolyte slurry was coated on a PET film and vacuum dried at 60° C. for 24 h to obtain a second solid electrolyte membrane with a thickness of 25 μm;
[0075] 7. Mix polysiloxane, PVDF-HFP and LiTFSI, and stir at high speed at room temperature to prepare a third solid electrolyte slurry; wherein the stirring rate is 1200 r / min, the stirring time is 30 min, the mass ratio of polysiloxane to PVDF-HFP is 1.5:1, and LiTFSI accounts for 80wt.% of the total mass of polysiloxane and PVDF-HFP;
[0076] 8. The third solid electrolyte slurry was coated on a PET film and vacuum dried at 60° C. for 24 h to obtain a third solid electrolyte membrane with a thickness of 5 μm;
[0077] 9. The first solid electrolyte membrane, the second solid electrolyte membrane and the third solid electrolyte membrane are stacked in sequence, and then hot-pressed at 120° C. and a pressure of 50 MPa for 30 min to obtain a sandwich-type composite solid electrolyte membrane.
[0078] Example 2
[0079] like Figure 1As shown, a composite solid electrolyte membrane includes a first solid electrolyte membrane 100 , a second solid electrolyte membrane 200 and a third solid electrolyte membrane 300 , wherein the second solid electrolyte membrane 200 is located between the first solid electrolyte membrane 100 and the third solid electrolyte membrane 300 .
[0080] The specific preparation method of the above composite solid electrolyte membrane is as follows:
[0081] 1. PEO, LiTFSI and NMP were mixed and stirred at high speed at room temperature to prepare a clear and transparent PEO glue; wherein the stirring rate was 1000 r / min, the stirring time was 30 min, and the mass ratio of PEO to LiTFSI was 1:1;
[0082] 2. LLTO (La 0.56 Li 0.33 TiO3) and NMP are mixed, ultrasonically dispersed for 30 minutes to form a uniform suspension, and mixed with PEO glue, and stirred at high speed at room temperature to obtain a first solid electrolyte slurry; wherein the stirring rate is 1200r / min, the stirring time is 30min, and the mass ratio of LLTO to PEO is 0.3:1;
[0083] 3. The first solid electrolyte slurry was coated on a PET film and vacuum dried at 60° C. for 24 h to obtain a first solid electrolyte membrane with a thickness of 4 μm;
[0084] 4. Mix NBR and p-xylene and stir to prepare a clear and transparent NBR glue;
[0085] 5. Li6PS5Br and p-xylene were mixed, ultrasonically dispersed for 30 minutes to form a uniform suspension, and mixed with NBR glue, and stirred thoroughly to obtain a second solid electrolyte slurry; wherein the mass ratio of Li6PS5Br to NBR was 26:1;
[0086] 6. The second solid electrolyte slurry was coated on a PET film and vacuum dried at 60° C. for 24 h to obtain a second solid electrolyte membrane with a thickness of 30 μm;
[0087] 7. Mix polysiloxane, PEO and LiTFSI, and stir at high speed at room temperature to prepare a third solid electrolyte slurry; wherein the stirring rate is 1200 r / min, the stirring time is 30 min, the mass ratio of polysiloxane to PEO is 1:1, and LiTFSI accounts for 50wt.% of the total mass of polysiloxane and PEO;
[0088] 8. The third solid electrolyte slurry was coated on a PET film and vacuum dried at 60° C. for 24 h to obtain a third solid electrolyte membrane with a thickness of 4 μm;
[0089] 9. The first solid electrolyte membrane, the second solid electrolyte membrane and the third solid electrolyte membrane are stacked in sequence, and then hot-pressed at 80° C. and a pressure of 25 MPa for 25 min to obtain a sandwich-type composite solid electrolyte membrane.
[0090] Example 3
[0091] like Figure 1 As shown, a composite solid electrolyte membrane includes a first solid electrolyte membrane 100 , a second solid electrolyte membrane 200 and a third solid electrolyte membrane 300 , wherein the second solid electrolyte membrane 200 is located between the first solid electrolyte membrane 100 and the third solid electrolyte membrane 300 .
[0092] The specific preparation method of the above composite solid electrolyte membrane is as follows:
[0093] 1. Mix PAN, LiTFSI and NMP and stir at high speed at room temperature to prepare a clear and transparent PAN glue solution; wherein the stirring rate is 1000 r / min, the stirring time is 30 min, and the mass ratio of PAN to LiTFSI is 1:0.5;
[0094] 2. LLZO and NMP were mixed, ultrasonically dispersed for 30 minutes to form a uniform suspension, and mixed with PAN glue, and stirred at high speed at room temperature to obtain the first solid electrolyte slurry; wherein the stirring rate was 1200 r / min, the stirring time was 30 minutes, and the mass ratio of LLZO to PAN was 0.5:1;
[0095] 3. The first solid electrolyte slurry was coated on a PET film and vacuum dried at 60° C. for 24 h to obtain a first solid electrolyte membrane with a thickness of 10 μm;
[0096] 4. Mix and stir SEBS and p-xylene to prepare a clear and transparent SEBS glue;
[0097] 5. Li3InCl6 and p-xylene were mixed, ultrasonically dispersed for 30 minutes to form a uniform suspension, and mixed with SEBS glue, and stirred thoroughly to obtain a second solid electrolyte slurry; wherein the mass ratio of Li3InCl6 to SEBS was 33:1;
[0098] 6. The second solid electrolyte slurry was coated on a PET film and vacuum dried at 60° C. for 24 h to obtain a second solid electrolyte membrane with a thickness of 28 μm;
[0099] 7. Mix polysiloxane, PAN and LiTFSI, and stir at high speed at room temperature to prepare a third solid electrolyte slurry; wherein the stirring rate is 1200 r / min, the stirring time is 30 min, the mass ratio of polysiloxane to PAN is 2:1, and LiTFSI accounts for 20 wt.% of the total mass of polysiloxane and PAN;
[0100] 8. The third solid electrolyte slurry was coated on a PET film and vacuum dried at 60° C. for 24 h to obtain a third solid electrolyte membrane with a thickness of 10 μm;
[0101] 9. The first solid electrolyte membrane, the second solid electrolyte membrane and the third solid electrolyte membrane are stacked in sequence, and then hot-pressed at 150° C. and a pressure of 20 MPa for 20 min to obtain a sandwich-type composite solid electrolyte membrane.
[0102] Example 4
[0103] like Figure 1 As shown, a composite solid electrolyte membrane includes a first solid electrolyte membrane 100 , a second solid electrolyte membrane 200 and a third solid electrolyte membrane 300 , wherein the second solid electrolyte membrane 200 is located between the first solid electrolyte membrane 100 and the third solid electrolyte membrane 300 .
[0104] The specific preparation method of the above composite solid electrolyte membrane is as follows:
[0105] 1. PVDF, LiTFSI and NMP were mixed and stirred at high speed at room temperature to prepare a clear and transparent PVDF glue; wherein the stirring rate was 1000 r / min, the stirring time was 30 min, and the mass ratio of PVDF to LiTFSI was 1:0.5;
[0106] 2. LAGP (Li 1.5 Al 0.5 Ge 1.5 (PO4)3) and NMP were mixed, ultrasonically dispersed for 30 minutes to form a uniform suspension, and mixed with PVDF glue, and stirred at high speed at room temperature to obtain a first solid electrolyte slurry; wherein the stirring rate was 1200r / min, the stirring time was 30min, and the mass ratio of LAGP to PVDF was 0.6:1;
[0107] 3. The first solid electrolyte slurry was coated on a PET film and vacuum dried at 60° C. for 24 h to obtain a first solid electrolyte membrane with a thickness of 8 μm;
[0108] 4. Mix HNBR and p-xylene and stir to prepare a clear and transparent HNBR glue;
[0109] 5. Li2S-P2S5 and p-xylene were mixed, ultrasonically dispersed for 30 minutes to form a uniform suspension, and mixed with HNBR glue, and stirred thoroughly to obtain a second solid electrolyte slurry; wherein the mass ratio of Li2S-P2S5 to HNBR was 24:1;
[0110] 6. The second solid electrolyte slurry was coated on a PET film and vacuum dried at 60° C. for 24 h to obtain a second solid electrolyte membrane with a thickness of 25 μm;
[0111] 7. Mix polysiloxane, PVDF and LiTFSI, and stir at high speed at room temperature to prepare a third solid electrolyte slurry; wherein the stirring rate is 1200 r / min, the stirring time is 30 min, the mass ratio of polysiloxane to PVDF is 1.2:1, and LiTFSI accounts for 50wt.% of the total mass of polysiloxane and PVDF;
[0112] 8. The third solid electrolyte slurry was coated on a PET film and vacuum dried at 60° C. for 24 h to obtain a third solid electrolyte membrane with a thickness of 8 μm;
[0113] 9. The first solid electrolyte membrane, the second solid electrolyte membrane and the third solid electrolyte membrane are stacked in sequence, and then hot-pressed at 120° C. and a pressure of 40 MPa for 10 min to obtain a sandwich-type composite solid electrolyte membrane.
[0114] Example 5
[0115] The composite solid electrolyte membrane provided in Example 5 is different from that in Example 1 only in that the thickness of the first solid electrolyte membrane and the third solid electrolyte membrane prepared in Example 5 are both 0.5 μm; the other conditions are the same as those in Example 1.
[0116] Example 6
[0117] The composite solid electrolyte membrane provided in Example 6 is different from that in Example 1 only in that the thickness of the first solid electrolyte membrane and the third solid electrolyte membrane prepared in Example 6 are both 11 μm; the other conditions are the same as those in Example 1.
[0118] Example 7
[0119] The composite solid electrolyte membrane provided in Example 7 is different from that in Example 1 only in that the hot pressing temperature in Example 7 is set to 170° C.; the other conditions are the same as those in Example 1.
[0120] Example 8
[0121] The composite solid electrolyte membrane provided in Example 8 is different from that in Example 1 only in that the hot pressing temperature in Example 8 is set to 60° C.; the other conditions are the same as those in Example 1.
[0122] Example 9
[0123] The composite solid electrolyte membrane provided in Example 9 is different from that in Example 1 only in that the hot pressing pressure in Example 9 is set to 60 MPa; the other conditions are the same as those in Example 1.
[0124] Example 10
[0125] The composite solid electrolyte membrane provided in Example 10 is different from that in Example 1 only in that the hot pressing pressure in Example 10 is set to 10 MPa; the other conditions are the same as those in Example 1.
[0126] Embodiment 11
[0127] The composite solid electrolyte membrane provided in Example 11 is different from that in Example 1 only in that the hot pressing time in Example 11 is set to 40 minutes; the other conditions are the same as those in Example 1.
[0128] Example 12
[0129] The composite solid electrolyte membrane provided in Example 12 is different from that in Example 1 only in that the hot pressing time in Example 12 is set to 5 minutes; the other conditions are the same as those in Example 1.
[0130] Comparative Example 1
[0131] A solid electrolyte membrane, the preparation method of which is as follows:
[0132] 1. PVDF-HFP, LiTFSI and NMP were mixed and stirred at high speed at room temperature to prepare a clear and transparent PVDF-HFP glue solution; wherein the stirring rate was 1000 r / min, the stirring time was 30 min, and the mass ratio of PVDF-HFP to LiTFSI was 1:0.5;
[0133] 2. LATP (Li 1.3 Al 0.3 Ti 1.7 (PO4)3) and NMP were mixed, ultrasonically dispersed for 30 minutes to form a uniform suspension, and mixed with PVDF-HFP glue, and stirred at high speed at room temperature to obtain a solid electrolyte slurry; wherein the stirring rate was 1200r / min, the stirring time was 30min, and the mass ratio of LATP to PVDF-HFP was 0.4:1;
[0134] 3. The solid electrolyte slurry was coated on a PET film and vacuum dried at 60°C for 24 h to obtain a solid electrolyte membrane with a thickness of 25 μm.
[0135] Comparative Example 2
[0136] A solid electrolyte membrane, the preparation method of which is as follows:
[0137] 1. Mix and stir SEBS and p-xylene to prepare a clear and transparent SEBS glue;
[0138] 2. Li6PS5Cl and p-xylene were mixed, ultrasonically dispersed for 30 minutes to form a uniform suspension, and mixed with SEBS glue, and stirred thoroughly to obtain a solid electrolyte slurry; wherein the mass ratio of Li6PS5Cl to SEBS was 33:1;
[0139] 3. The solid electrolyte slurry was coated on a PET film and vacuum dried at 60°C for 24 h to obtain a solid electrolyte membrane with a thickness of 25 μm.
[0140] Comparative Example 3
[0141] A solid electrolyte membrane, the preparation method of which is as follows:
[0142] 1. Mix polysiloxane, PVDF-HFP and LiTFSI, and stir them at high speed at room temperature to prepare a solid electrolyte slurry; wherein the stirring rate is 1200r / min, the stirring time is 30min, the mass ratio of polysiloxane to PVDF-HFP is 1.5:1, and LiTFSI accounts for 80wt.% of the total mass of polysiloxane and PVDF-HFP;
[0143] 2. The solid electrolyte slurry was coated on a PET film and vacuum dried at 60°C for 24 h to obtain a solid electrolyte membrane with a thickness of 25 μm.
[0144] Solid electrolyte membrane performance test
[0145] The solid electrolyte membranes prepared in the above-mentioned Examples 1-12 and Comparative Examples 1-3 were used as test samples and the following tests were performed.
[0146] Test method:
[0147] 1. Mechanical strength: Use a universal tensile testing machine to test the mechanical strength of each sample;
[0148] 2. Thermal shrinkage test: Place the sample in a 130°C constant temperature box and heat for 30 minutes. Test the length change of the sample before and after heating. Thermal shrinkage = (L1-L2) / L1×100%, L1: length before heating; L2: length after heating;
[0149] 3. Ionic conductivity: The sample was cut into original sheets with a diameter of 10 mm, and then stainless steel sheets were used as ion blocking electrodes and placed on both sides of the original sheets to make ion blocking cells. The EIS test was performed using an electrochemical workstation with a frequency range of 1 to 10 6Hz, amplitude 10mV, the Nyquist spectrum is obtained after the test, and the ionic conductivity of the solid electrolyte membrane is calculated by the formula σ=L / (R*A), L is the thickness of the solid electrolyte membrane, A is the effective area of the solid electrolyte membrane, and R is the bulk resistance of the solid electrolyte membrane.
[0150] The above test results are shown in Table 1.
[0151] Table 1
[0152]
[0153]
[0154] Application Example 1
[0155] like Figure 2 As shown, an all-solid-state battery includes a positive electrode sheet 400, a negative electrode sheet 500 and a composite solid electrolyte membrane prepared in Example 1, wherein the first solid electrolyte membrane 100 is close to the positive electrode sheet 400, and the third solid electrolyte membrane 300 is close to the negative electrode sheet 500.
[0156] The specific preparation method of the above-mentioned all-solid-state battery is as follows:
[0157] Preparation of positive electrode sheet: NCM811 positive electrode active material, Li6PS5Cl solid electrolyte, VGCF conductive agent and SEBS binder are added to the solvent in a mass ratio of 80:20:2:3, and mixed thoroughly to obtain positive electrode slurry; the positive electrode slurry is evenly coated on aluminum foil, and the positive electrode sheet is obtained through baking, rolling, striping and die-cutting processes;
[0158] Negative electrode preparation: lithium metal electrode is used;
[0159] Assembly of the all-solid-state battery: The positive electrode sheet, the composite solid electrolyte membrane prepared in Example 1, and the negative electrode sheet are assembled by lamination, hot pressing, and isostatic pressing to prepare an all-solid-state battery.
[0160] Application Example 2-12
[0161] The all-solid-state batteries provided in Application Examples 2-12 differ from Application Example 1 only in that the composite solid electrolyte membrane prepared in Example 1 is replaced by the composite solid electrolyte membrane prepared in Examples 2-12; the other conditions are the same as those in Application Example 1.
[0162] Comparative Application Examples 1-3
[0163] The all-solid-state batteries provided in comparative application examples 1-3 differ from application example 1 only in that the composite solid electrolyte membrane prepared in example 1 is replaced by the solid electrolyte membrane prepared in comparative examples 1-3, respectively; the other conditions are the same as those in application example 1.
[0164] All-solid-state battery performance test
[0165] The all-solid-state batteries prepared in the above-mentioned application examples 1-12 and comparative application examples 1-3 were used as test samples and the following tests were carried out.
[0166] Test method:
[0167] 1. First coulombic efficiency: At room temperature, the all-solid-state battery is charged and discharged for the first time at a rate of 0.1C. The first coulombic efficiency = first discharge specific capacity / first charge specific capacity × 100%;
[0168] 2. Cycle performance: At room temperature, the all-solid-state battery is tested for cycle performance at a rate of 0.3C. The life span ends when the capacity retention rate reaches 80%.
[0169] The above test results are shown in Table 2.
[0170] Table 2
[0171]
[0172]
[0173] From the test results in Tables 1 and 2 above, it can be seen that the composite solid electrolyte membrane of the present invention has good mechanical strength, good flexibility, thermal stability and ionic conductivity; the all-solid-state battery prepared using the composite solid electrolyte membrane of the present invention has good safety performance and charge and discharge cycle performance.
[0174] The preferred embodiments of the present invention are specifically described above, but the invention is not limited to the embodiments. Those skilled in the art may make various equivalent modifications or substitutions without violating the spirit of the invention. These equivalent modifications or substitutions are all included in the scope defined by the claims of this application.
Claims
1. An all-solid-state battery, characterized in that: The all-solid-state battery comprises a positive electrode sheet, a negative electrode sheet and a composite solid electrolyte membrane; The composite solid electrolyte membrane comprises a first solid electrolyte membrane, a second solid electrolyte membrane and a third solid electrolyte membrane, wherein the second solid electrolyte membrane is located between the first solid electrolyte membrane and the third solid electrolyte membrane; The first solid electrolyte membrane is close to the positive electrode sheet, and the third solid electrolyte membrane is close to the negative electrode sheet; The raw materials for preparing the first solid electrolyte membrane consist of polymer A, lithium salt, a first solvent and a first solid electrolyte; The raw materials for preparing the second solid electrolyte membrane consist of a B polymer, a second solvent and a second solid electrolyte; The raw materials for preparing the third solid electrolyte membrane are composed of polysiloxane, A polymer and lithium salt; The A polymer is at least one of polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene, polymethyl methacrylate, polyethylene oxide and polyacrylonitrile; The first solid electrolyte comprises an oxide solid electrolyte; The B polymer is at least one of styrene-butadiene-styrene elastomer, styrene-butadiene-styrene block copolymer, nitrile rubber, hydrogenated nitrile rubber, butadiene rubber, natural rubber and aliphatic polycarbonate; The second solid electrolyte includes a sulfide solid electrolyte and / or a halide solid electrolyte.
2. The all-solid-state battery according to claim 1, characterized in that: The oxide solid electrolyte includes Li 1+ a Al a Ti 2-a (PO4)3、Li 1+b Al b Ge 2-b (PO4)3, La 2 / 3-c Li 3c TiO3、La 0.56 Li 0.33+d Ti 1-d Al d O3、Li7La3Zr2O 12 , Li 6.4 Ln3Z 1.4 Ta 0.6 O 12 and Li 6.75 Ln3Z 1.75 Nb 0.25 O 12 At least one of; wherein, 0≤a≤0.5, 0≤b≤0.65, 0.04 <c<0.17,0≤d≤0.06。 3. The all-solid-state battery according to claim 1, characterized in that: The second solid electrolyte includes Li6PS5Cl, Li6PS5Br, Li2S-P2S5, Li4GeS4, Li 10 GeP2S 12 , Li 9.54 Si 1.74 P 1.44 S 11.7 Cl 0.3 、Li3PS4、Li7P3S 11 、Li3YCl6、Li3InCl6、Li 2-2x Mn 1+x Cl4、Li 2-2x Fe 1+x Cl4、Li 2-2x Mg 1+x Cl4、Li 2-2x Mn 1+x Br4 and Li 2-2x Mg 1+x At least one of Br4; wherein 0≤x≤0.
33.
4. The all-solid-state battery according to claim 1, characterized in that: The lithium salt includes at least one of LiTFSI, LiFSI, Li(CF3SO2)3C, LiC4F9SO3, LiN(SO2CF2CF3)2, LiB(C2O4)2, LiBF4, LiBF3(C2F5), LiSCN, LiN(CN)2, LiDFOB, LiODFB, LiN(SO2F)2, LiCF3SO3, LiClO4, LiAsF6 and LiSbF6.
5. The all-solid-state battery according to claim 1, characterized in that: The first solvent includes at least one of N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, acetonitrile and dimethyl sulfoxide; and / or the second solvent includes at least one of toluene, p-xylene, dichloromethane, dichloroethane, dichloropropane, dibromomethane, dibromoethane, dibromopropane, cyclohexane, n-heptane, n-decane, n-octane, anisole, butyl butyrate and benzyl acetate.
6. The all-solid-state battery according to claim 1, characterized in that: The thickness of the first solid electrolyte membrane is 1-10 μm; and / or the thickness of the second solid electrolyte membrane is 15-40 μm; and / or the thickness of the third solid electrolyte membrane is 1-10 μm.
7. The all-solid-state battery according to claim 1, characterized in that: The composite solid electrolyte membrane is prepared by a preparation method comprising the following steps: The first solid electrolyte membrane, the second solid electrolyte membrane and the third solid electrolyte membrane are stacked and then subjected to hot pressing to obtain a composite solid electrolyte membrane.
8. The all-solid-state battery according to claim 7, characterized in that: The temperature of the hot pressing is 80-150° C.; and / or, the time of the hot pressing is 10-30 min; and / or, the pressure of the hot pressing is 20-50 MPa.