Cryogenic Pressure Regulating Composite Casting Method for Light Alloy Cabin of Aerospace Vehicle

By using a cryogenic sand mold pressure-adjusting composite casting method, problems such as oxidation and air absorption in gravity casting of light alloy cabins for aerospace vehicles have been solved, enabling rapid prototyping and performance improvement of high-precision, large-size thin-walled castings.

CN118385535BActive Publication Date: 2026-11-17NANJING UNIV OF AERONAUTICS & ASTRONAUTICS
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410551846.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-07
Publication Date
2026-11-17
Estimated Expiration
2044-05-07

AI Technical Summary

Technical Problem

Light alloy cabins for aerospace vehicles are prone to defects such as oxidation, air absorption, air entrapment, and slag inclusions in conventional gravity casting, making it difficult to achieve rapid response to structural design iterations and high-precision forming.

Method used

A cryogenic sand mold pressure-regulating composite casting method is adopted. Cryogenic sand molds are prepared by low-temperature CNC machining or cryogenic printing. Combined with vacuum melting and pressure-regulating casting, the process of molten metal filling is controlled, and the solidification process is regulated by liquid nitrogen cooling, so as to achieve precise monitoring and rapid forming.

Benefits of technology

It has improved the yield and mechanical properties of lightweight alloy cabins for aerospace vehicles, shortened the technology development cycle, reduced casting defects, and improved the response speed and stability of the process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118385535B_ABST
    Figure CN118385535B_ABST
Patent Text Reader

Abstract

This invention discloses a cryogenic pressure-regulating composite casting method for lightweight alloy cabins of aerospace vehicles, belonging to the interdisciplinary field of mechanical manufacturing automation and sand casting technology. The invention constructs a corresponding three-dimensional model of a cryogenic sand mold and obtains the mold through machining. The manufactured cryogenic sand mold of the aerospace vehicle cabin is loaded into the upper pressure cylinder of a designed cryogenic sand mold pressure-regulating casting system, while the lower pressure cylinder is filled with pre-prepared alloy raw materials, ceramic riser pipes, and ceramic filters. The upper and lower pressure cylinders are then closed, and a vacuum is simultaneously drawn from both cylinders. Gas washing is performed inside the upper and lower cylinders to reduce the oxygen content and minimize the formation of oxide inclusions during subsequent pouring. This invention solves problems such as sand flushing, gas entrapment, and oxide inclusions in the gravity casting process of lightweight alloys using cryogenic sand molds, enabling rapid response in the design and manufacturing of aerospace vehicle cabins and promoting the innovative and green development of lightweight alloy casting technology.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the interdisciplinary field of differential pressure casting and cryogenic sand casting technology, specifically involving a cryogenic pressure regulating composite casting forming method for lightweight alloy cabins of aerospace vehicles. Background Technology

[0002] The rapid development of the aerospace industry has led to an increasing demand for weight reduction in spacecraft. The structural design of key components for spacecraft is showing a trend towards integration. Due to the complexity of the designed spacecraft structures, key components such as the fuselage and guide vanes are often integrally formed using casting methods. The design of spacecraft fuselage structures involves rapid iteration, with most requirements being for single-piece, small-batch production. This necessitates casting solutions that possess key characteristics such as fast response time, short iteration time, and low cost.

[0003] Frozen sand casting technology is a green casting technology that uses water as a sand mold binder to freeze the sand mold in a low-temperature environment. High-precision frozen sand molds are obtained through additive and subtractive material techniques, and molten metal is poured in to obtain the casting. It features low manufacturing cost, fast process design response speed, and environmental friendliness.

[0004] Spacecraft cabins are mostly made of lightweight alloys, such as titanium alloys, aluminum-lithium alloys, and rare earth magnesium alloys. These alloys have high melt activity and are prone to defects such as oxidation, gas absorption, gas entrapment, and slag inclusion during conventional gravity casting filling processes, which directly affect the yield of spacecraft cabins.

[0005] Pressure-controlled casting is a casting method that applies pressure during the filling and solidification of molten metal, precisely controlling the process to effectively eliminate porosity and shrinkage defects, resulting in denser and more uniform castings. Compared to traditional gravity casting, pressure-controlled casting can produce lightweight alloy castings with various complex shapes and high precision requirements, such as thin-walled structures, slender components, and castings with internal cavities. The rapid cooling and solidification process in pressure-controlled casting can also improve the mechanical properties of the castings to some extent.

[0006] The cryogenic pressure-regulating composite casting method for lightweight alloy spacecraft cabins combines cryogenic sand casting and pressure-regulating casting methods. This method can quickly respond to the iterative needs of structural design for spacecraft cabins, broaden the applicability of cryogenic sand casting, and achieve precise control of the filling and solidification process of large-size integrated thin-walled lightweight alloy spacecraft cabins. This results in high-performance spacecraft cabins and promotes the rapid development of the aerospace industry. Summary of the Invention

[0007] To address the aforementioned problems, this invention discloses a cryogenic pressure-regulating composite casting method for lightweight alloy cabins of aerospace vehicles. This method solves problems such as sand flushing, air entrapment, and oxide inclusions in the cryogenic sand mold gravity casting process of lightweight alloys, resulting in large-size thin-walled aerospace vehicle cabin castings with excellent mechanical properties. This enables rapid response in the design and manufacturing of aerospace vehicle cabins and promotes the development of lightweight alloy casting technology.

[0008] This invention discloses a cryogenic pressure-regulating composite casting method for lightweight alloy spacecraft cabins. Based on the structural requirements of the spacecraft cabin, a corresponding casting process is designed, and a corresponding three-dimensional model of a cryogenic sand mold is constructed. The cryogenic sand mold is obtained through low-temperature CNC machining or cryogenic printing. The manufactured cryogenic sand mold of the spacecraft cabin is loaded into the upper pressure cylinder of the designed cryogenic sand mold pressure-regulating casting system. Pre-prepared alloy raw materials, ceramic riser pipes, and ceramic filters are loaded into the lower pressure cylinder. The upper and lower pressure cylinders are closed, and vacuum is simultaneously drawn from both cylinders. After the upper and lower cylinders reach the set vacuum level, a certain flow rate of argon gas is injected, and vacuum is continued to purge the gas inside the upper and lower cylinders, reducing the oxygen content and minimizing the formation of oxide inclusions during subsequent pouring. After purge, the lower cylinder melting furnace is powered on to melt the prepared alloy raw materials. Once the alloy melt reaches the set pouring temperature, the pressurization system injects argon gas into the lower cylinder to increase its pressure. When the lower cylinder reaches the preset pressure, the upper and lower cylinders are slowly connected. Under pressure, the molten metal slowly flows into the riser pipe. Subsequently, as the pressure in the lower cylinder increases, the molten metal flows into the cryogenic sand mold cavity. As the molten metal continues to fill the mold, the temperature measurement device in the cryogenic sand mold monitors the mold temperature. When the mold temperature exceeds the preset temperature (-5℃), the liquid nitrogen cooling system activates, rapidly lowering the mold temperature and maintaining the strength of the cryogenic sand mold. Simultaneously, the cooling effect of liquid nitrogen also increases the solidification rate of the molten metal, improving the mechanical properties of the final casting to some extent. During the filling process, a stable pressure difference is maintained between the upper and lower cylinders, effectively feeding the casting. Once the casting has solidified, the pressure difference between the upper and lower cylinders is broken, and the unsolidified molten metal flows back into the crucible. After overall cooling, the cylinders are opened and the sand is removed, yielding the chamber casting.

[0009] To achieve the above objectives, the frozen sand mold pressure regulating casting system of the present invention is carried out according to the following steps:

[0010] Step 1: Design the corresponding casting process based on the structural characteristics of the aerospace vehicle cabin, and process the corresponding cryogenic sand mold for the aerospace vehicle cabin.

[0011] Step 2: Place the processed aerospace vehicle cabin cryogenic sand mold into the upper pressure cylinder of the cryogenic sand mold pressure regulating casting system, and close the upper pressure cylinder;

[0012] Step 3: Add the prepared alloy raw materials to the crucible in the lower pressure cylinder of the cryogenic sand mold pressure regulating casting system, install the corresponding ceramic riser pipe and ceramic filter screen, and close the lower pressure cylinder;

[0013] Step 4: Evacuate the upper and lower cylinders to reach the set vacuum level (0.1MPa-0.5MPa), then introduce argon gas into the furnace and continue evacuating the vacuum. When the set vacuum level is reached for the second time, the furnace cavity cleaning process of the upper and lower cylinders is completed. The gas suction process helps to reduce the oxygen content of the upper and lower cylinders and reduce the possible formation of oxide inclusions during subsequent casting.

[0014] Step 5: Close the valve connecting the upper and lower cylinders, turn on the lower cylinder melting heating component to heat and melt the alloy raw materials in the crucible;

[0015] Step 6: When the alloy temperature reaches the set temperature, increase the pressure in the lower cylinder to (0.1MPa-1.5MPa) and hold it at that temperature for a period of time. The pressurization and heat holding process helps to remove the gas adsorbed in the original alloy melt and reduces the possibility of subsequent casting defects.

[0016] Step 7: After the heat preservation process is completed, the pressure in the lower cylinder is increased. As the pressure in the lower cylinder increases, the molten metal rises continuously in the riser pipe under the pressure.

[0017] Step 8: As the pressure in the lower cylinder continues to increase, the molten metal rises and melts the plastic separating film. The molten metal is then poured into the frozen sand mold cavity and filled through the designed slit-type gating system.

[0018] Step 9: While the molten metal is filling the mold, the temperature sensor inside the frozen sand mold monitors the temperature of the frozen sand mold in real time and obtains the filling status of the casting. When the sand mold temperature exceeds the set temperature (-5℃), the liquid nitrogen valve is opened and liquid nitrogen is introduced into the cooling pipe. The frozen sand mold is directly cooled through the nozzle to regulate the temperature state of the frozen sand mold and control the solidification process of the casting.

[0019] Step 10: After the filling process is completed, the lower cylinder maintains a stable pressure and forms a stable pressure difference with the upper cylinder, which increases the feeding capacity of the molten metal, reduces casting defects, and improves the performance of the casting.

[0020] Step 11: Clean the loose sand around the casting using a negative pressure device, spray the casting surface with a low-temperature medium such as liquid nitrogen, and use the liquid nitrogen spray to quickly cool the casting so that it forms a directional solidification from the end of the casting to the gate, thereby improving the mechanical properties of the casting.

[0021] Step 12: After the casting has solidified, the gas valve connecting the upper and lower cylinders is slowly opened, connecting the two cylinders. The unsolidified molten metal flows back to the lower cylinder crucible under pressure.

[0022] Step 13: Once the temperature of the upper and lower cylinders drops below 50°C, slowly open the air valves connecting the upper and lower cylinders to the outside air to depressurize the system.

[0023] Step 14: Open the upper cylinder and perform the sand cleaning process to obtain a frozen sand mold low-pressure casting;

[0024] Step 15: Open the lower cylinder, clean the crucible, and replace the riser tube and filter screen components to prepare for the next use.

[0025] Furthermore, the casting production methods targeted by this system are not limited to pressure-adjusting casting. By controlling the pressure process curves of the upper and lower cylinders, it can realize casting methods under various external forces, such as low-pressure casting, differential pressure casting, and pressure-adjusting casting of light alloy castings using frozen sand molds.

[0026] Furthermore, the refrigerant can be a cooling substance such as liquid nitrogen or dry ice. By measuring the temperature of the frozen sand mold, the solidification process of the frozen sand casting can be monitored. By spraying liquid nitrogen into the frozen sand mold during the solidification process, the shape and integrity of the frozen sand mold can be maintained. At the same time, the amount of liquid nitrogen sprayed can control the cooling rate of the casting, thereby achieving precise control of the solidification process of the casting, realizing the overall layer-by-layer solidification of the casting, and improving the overall mechanical properties of the casting.

[0027] The beneficial effects of this invention are:

[0028] 1. This invention improves the quality of lightweight alloy cabin castings by precisely controlling the temperature field distribution of the frozen sand mold and thus the solidification process. By measuring the temperature of the frozen sand mold during molten metal pouring, precise monitoring of the solidification process is achieved. During solidification, liquid nitrogen is sprayed onto the frozen sand mold, allowing low-temperature air to rapidly pass through the mold pores under negative pressure, maintaining the mold's shape and integrity. The cooling rate of the casting is controlled by the amount of liquid nitrogen injected, enabling precise regulation of the solidification process. The casting solidifies layer by layer, improving its overall mechanical properties.

[0029] 2. This invention shortens the development cycle of lightweight alloy cabin technology for aerospace vehicles by coupling cryogenic sand casting and pressure-regulated casting, reducing defects in cabin castings and improving process yield and stability. Traditional cryogenic sand casting for lightweight alloy castings suffers from the difficulty in controlling the molten metallurgical quality during the transfer and pouring process due to the lightweight alloy's tendency to absorb gas, easily leading to defects such as oxidation inclusions. Cabin castings are mostly large-sized, thin-walled parts; under gravity casting conditions, the high cooling rate of the cryogenic sand mold results in generally poor metal fluidity, easily leading to defects such as incomplete filling and cold shuts. Under pressure-regulated casting conditions, the combination of vacuum melting and negative pressure degassing ensures better metallurgical quality in the molten metal, and the melting and pouring process is continuous, greatly reducing casting defects caused by metal oxidation and gas absorption. With the aid of pressure-regulated casting, the molten metal fills the mold smoothly, and the suction effect of the negative pressure greatly enhances the filling capacity of the molten metal, solving many defects such as incomplete filling and cold shuts caused by insufficient molten metal fluidity.

[0030] 3. Compared with traditional sand casting, the high cooling rate and self-collapse effect of the frozen sand mold can improve the mechanical properties of the casting, while reducing the residual stress caused by obstructed shrinkage between the light alloy casting and the rigid mold, reducing the stress deformation of thin-walled castings, and improving the quality of the casting. Attached Figure Description

[0031] Figure 1 Schematic diagram of a cryogenic sand mold pressure regulating casting system;

[0032] Figure 2 Schematic diagram of the main components of a cryogenic sand mold pressure regulating casting furnace;

[0033] Figure 3 This is a schematic diagram of the pressure and mold temperature process curves for low-pressure casting with forced cooling, as per the present invention.

[0034] List of reference numerals in the attached diagram:

[0035] 1- Cryogenic sand mold pressure regulating casting furnace; 2- Vacuum pressure gauge one; 3- Pneumatic ball valve one; 4- Pneumatic ball valve two; 5- Vacuum buffer tank; 6- Shut-off valve; 7- Pneumatic ball valve three; 8- Vacuum pressure gauge two; 9- Digital combination valve one; 10- Pneumatic ball valve four; 11- Pressure reducing valve; 12- Gas storage tank; 13- Cryogenic sand mold temperature acquisition module; 14- Digital combination valve two; 15- Liquid nitrogen storage tank; 16- Pneumatic ball valve five. 1-01-Upper pressure cylinder; 1-02-Upper cylinder pressure signal acquisition hole; 1-03-Upper cylinder inlet and outlet; 1-04-Pressure relief valve; 1-05-Liquid nitrogen cooling device; 1-06-Aerospace vehicle cabin cryogenic sand mold system; 1-07-Cryogenic sand mold temperature sensor; 1-08-Ceramic filter screen one; 1-09-Liquid nitrogen connecting pipe; 1-10-Middle partition; 1-11-Liquid riser pipe; 1-12-Ceramic filter screen two; 1-13-Lower pressure cylinder pressure signal acquisition hole; 1-14-Lower pressure cylinder inlet and outlet; 1-15-Lower pressure cylinder; 1-16-Heating element; 1-17-Furnace lining; 1-18-Crucible; 1-19-Electrode assembly; 1-20-Thermocouple assembly; 1-21-Plastic separator film. Detailed Implementation

[0036] The present invention will be further illustrated below with reference to the accompanying drawings and specific embodiments. It should be understood that the following specific embodiments are for illustrative purposes only and are not intended to limit the scope of the invention. It should be noted that the terms "front," "rear," "left," "right," "up," and "down" used in the following description refer to directions in the accompanying drawings, and the terms "inner" and "outer" refer to directions toward or away from the geometric center of a specific component, respectively.

[0037] This invention proposes a cryogenic pressure-regulating composite casting method for lightweight alloy cabins of aerospace vehicles, such as... Figure 1 As shown.

[0038] Step 1: Design the corresponding casting process based on the structural characteristics of the aerospace vehicle cabin, and process the corresponding aerospace vehicle cabin cryogenic sand mold system 1-06;

[0039] Step 2: Place the processed aerospace vehicle cabin cryogenic sand mold 1-06 into the upper pressure cylinder 1-01 of the cryogenic sand mold pressure regulating casting system, and close the upper pressure cylinder 1-01;

[0040] Step 3: Add the prepared alloy raw materials to the crucible 1-18 in the lower pressure cylinder 1-15 of the cryogenic sand mold pressure regulating casting system, install the corresponding ceramic riser pipe 1-11 and ceramic filter screen 1-12, and close the lower pressure cylinder 1-15;

[0041] Step 4: Open pneumatic ball valve 1 (3), pneumatic ball valve 2 (4), and pneumatic ball valve 5 (16) and close pneumatic ball valve 3 (7) and pneumatic ball valve 4 (10) to achieve the set vacuum level. Then, introduce argon gas into the furnace and continue to evacuate the vacuum. When the set vacuum level is reached for the second time, the furnace cavity cleaning process of the upper and lower cylinders is completed. The gas suction process helps to reduce the oxygen content of the upper and lower cylinders and reduce the possible formation of oxide inclusions during the subsequent casting process.

[0042] Step 5: Close the upper and lower cylinders 1-01 and 1-15, connect the pneumatic ball valve 16, and turn on the lower cylinder melting heating assembly 1-20 to heat and melt the alloy raw materials in the crucible 1-18;

[0043] Step 6: When the alloy temperature reaches the set temperature, open the pneumatic ball valve 410, fill with argon gas, increase the pressure of the lower cylinder 1-15 to P1, and keep it at the temperature for a period of time; the pressurization and heat preservation process helps to remove the gas adsorbed in the original alloy melt and reduce the possibility of subsequent casting defects.

[0044] Step 7: After the heat preservation process is completed, increase the pressure in the lower cylinder 1-15. As the pressure in the lower cylinder 1-15 increases, the molten metal will rise continuously in the riser pipe 1-11 under the action of pressure.

[0045] Step 8: As the pressure in the lower cylinder 1-15 continues to increase, the molten metal rises and melts the plastic separating film 1-21. The molten metal is then poured into the frozen sand mold cavity 1-06, and the molten metal filling process is carried out through the designed slit-type gating system.

[0046] Step 9: While the molten metal is filling the mold, the temperature sensor 1-08 inside the frozen sand mold monitors the temperature of the frozen sand mold in real time and obtains the filling status of the casting. When the sand mold temperature exceeds the set temperature, the liquid nitrogen valve 14 is opened and liquid nitrogen is introduced into the cooling pipe. The frozen sand mold 1-06 is directly cooled through the nozzle 1-05 to regulate the temperature state of the frozen sand mold and control the solidification process of the casting.

[0047] Step 10: After the filling process is completed, the lower cylinder 1-15 maintains a stable pressure and forms a stable pressure difference with the upper cylinder 1-01, which increases the feeding capacity of the molten metal, reduces casting defects, and improves the performance of the casting.

[0048] Step 11: The high temperature of the casting destroys the frozen mold. Open the pneumatic ball valve 24 to increase the negative pressure of the upper cylinder. Under the action of negative pressure, the frozen sand mold gradually breaks down and the casting gradually emerges. Spray liquid nitrogen and other low-temperature media on the surface of the casting through liquid nitrogen nozzle 1-05. The rapid cooling by spraying liquid nitrogen causes the casting to form a directional solidification from the end of the casting to the gate, which improves the mechanical properties of the casting.

[0049] Step 12: After the casting has solidified, the pneumatic ball valve 16 connecting the upper and lower cylinders 1-01 and 1-15 is slowly opened, connecting the two cylinders. The unsolidified molten metal flows back to the lower cylinder crucible 1-18 under pressure.

[0050] Step 13: When the temperature of the furnace chamber of the frozen sand mold pressure-regulating casting furnace 1 drops below 100 degrees Celsius, slowly open the upper and lower cylinders and the external air valves to depressurize the system.

[0051] Step 14: Open the upper cylinder 1-01 to perform the sand cleaning process and obtain the frozen sand mold low-pressure casting;

[0052] Step 15: Open the lower cylinder 1-15, clean the crucible 1-18, and replace the riser tube 1-11 and filter screen 1-12 to prepare for the next use.

[0053] The specific implementation steps of the low-pressure casting enhanced cooling method of the present invention are as follows:

[0054] Step 1: Machin the frozen sand mold required for the corresponding casting, and load the sand mold into the upper pressure cylinder, then close the upper pressure cylinder;

[0055] Step 2: Add the prepared alloy raw materials to the crucible in the lower pressure cylinder of the cryogenic sand mold pressure regulating casting system, install the corresponding ceramic riser pipe and ceramic filter screen, and close the lower pressure cylinder;

[0056] Step 4: Evacuate the upper and lower cylinders to a set vacuum level of 0.1MPa to 0.5MPa, then introduce argon gas as a protective gas into the furnace and continue evacuating. When the set vacuum level is reached for the second time, the furnace cavity cleaning process of the upper and lower cylinders is completed. The gas suction process helps to reduce the oxygen content of the upper and lower cylinders.

[0057] Step 5: Close the valve connecting the upper and lower cylinders, turn on the lower cylinder melting heating component to heat and melt the alloy raw materials in the crucible;

[0058] Step 6: When the alloy temperature reaches the set temperature, increase the pressure in the lower cylinder to 0.1MPa~1.5MPa and hold it at that temperature for a period of time. The pressurization and heat holding process helps to remove the gas adsorbed in the original alloy melt and reduces the possibility of subsequent casting defects.

[0059] Step 7: The heat preservation process is complete. Follow the instructions... Figure 3 As required by the pressure process curve shown, the pressure of the lower cylinder is increased, and the molten metal rises continuously in the riser tube under the pressure.

[0060] Step 8: As the pressure in the lower cylinder continues to increase, the molten metal melts the plastic separating film and is then poured into the frozen sand mold cavity. The molten metal filling process is carried out through the designed slit gating system.

[0061] Step 9: While the molten metal is filling the mold, a temperature sensor inside the cryogenic sand mold monitors the temperature of the cryogenic sand mold in real time and obtains the filling status of the casting. A liquid nitrogen cooling device ensures that the sand mold temperature is maintained according to the specified parameters. Figure 3 The set sand mold temperature curve changes; pressure and temperature are controlled in a coordinated manner to ensure the implementation of low-pressure casting and forced cooling processes;

[0062] Step 10: After the filling process is completed, the lower cylinder maintains a stable pressure and forms a stable pressure difference with the upper cylinder, which increases the feeding capacity of the molten metal, reduces casting defects, and improves the performance of the casting.

[0063] Step 11: Clean the loose sand around the casting using a negative pressure device. At this time, liquid nitrogen is used to force-cool the casting to achieve rapid solidification.

[0064] Step 12: After the casting has solidified, the gas valve connecting the upper and lower cylinders is slowly opened, connecting the two cylinders. The unsolidified molten metal flows back to the lower cylinder crucible under pressure.

[0065] Step 13: Once the temperature of the upper and lower cylinders drops below 50°C, slowly open the air valves connecting the upper and lower cylinders to the outside air to depressurize the system.

[0066] Step 14: Open the upper cylinder and perform the sand cleaning process to obtain a frozen sand mold low-pressure casting;

[0067] Step 15: Open the lower cylinder, clean the crucible, and replace the riser tube and filter screen components to prepare for the next use.

[0068] The technical means disclosed in this invention are not limited to those disclosed in the above embodiments, but also include technical solutions composed of any combination of the above technical features.

Claims

1. A method for cryogenic pressure-regulating composite casting of a light alloy cabin for aerospace vehicles, characterized in that: Includes the following steps: Step 1: Design the corresponding casting process based on the structural characteristics of the aerospace vehicle cabin, and process the corresponding cryogenic sand mold for the aerospace vehicle cabin. Step 2: Place the processed aerospace vehicle cabin cryogenic sand mold into the upper pressure cylinder of the pressure regulating casting system equipped with temperature detection and sensing, and then close the upper pressure cylinder; Step 3: Add the prepared alloy raw materials to the crucible in the lower pressure cylinder of the cryogenic sand mold pressure regulating casting system, install the corresponding ceramic riser pipe and ceramic filter screen, and close the lower pressure cylinder; Step 4: Evacuate the upper and lower cylinders to reach the set vacuum level, introduce argon gas as a protective gas into the furnace, and continue to evacuate the vacuum level. When the set vacuum level is reached for the second time, the gas washing process of the upper and lower cylinder furnace chambers is completed. The gas washing process helps to reduce the oxygen content of the upper and lower cylinders. Step 5: Close the valve connecting the upper and lower cylinders, turn on the lower cylinder melting heating component to heat and melt the alloy raw materials in the crucible; Step 6: When the alloy temperature reaches the set temperature, increase the pressure in the lower cylinder to 0.1MPa~1.5MPa and hold it at that temperature for a period of time; The pressurization and heat preservation process helps to remove the gas adsorbed in the original alloy melt, reducing the possibility of subsequent casting defects. Step 7: After the heat preservation process is completed, the pressure in the lower cylinder is increased. As the pressure in the lower cylinder increases, the molten metal rises continuously in the riser pipe under the pressure. Step 8: As the pressure in the lower cylinder continues to increase, the molten metal rises and melts the plastic film. The molten metal is then poured into the frozen sand mold cavity and filled through the designed slit gating system. Step 9: While the molten metal is filling the mold, the temperature sensor inside the frozen sand mold monitors the temperature of the frozen sand mold in real time and obtains the filling status of the casting. When the sand mold temperature exceeds the set temperature of -5℃ to 5℃, the liquid nitrogen valve is opened and liquid nitrogen is introduced into the cooling pipe. The frozen sand mold is directly cooled through the nozzle to regulate the temperature state of the frozen sand mold and control the solidification process of the casting. Step 10: After the filling process is completed, the lower cylinder maintains a stable pressure and forms a stable pressure difference with the upper cylinder, which increases the feeding capacity of the molten metal, reduces casting defects, and improves the performance of the casting. Step 11: The high temperature of the casting destroys the frozen mold. Open the pneumatic ball valve two to increase the negative pressure of the upper cylinder. Under the action of negative pressure, the frozen sand mold gradually breaks down and the casting gradually emerges. Spray liquid nitrogen cryogenic medium onto the surface of the casting through the liquid nitrogen nozzle. The rapid cooling by spraying liquid nitrogen causes the casting to form a directional solidification from the end of the casting to the gate, which improves the mechanical properties of the casting. Step 12: After the casting has solidified, the gas valve connecting the upper and lower cylinders is slowly opened, connecting the two cylinders. The unsolidified molten metal flows back to the lower cylinder crucible under pressure. Step 13: Once the temperature of the upper and lower cylinders drops below 50°C, slowly open the air valves connecting the upper and lower cylinders to the outside air to depressurize the system. Step 14: Open the upper cylinder and perform the sand cleaning process to obtain a frozen sand mold low-pressure casting; Step 15: Open the lower cylinder, clean the crucible, and replace the riser pipe and filter screen components to prepare for the next use; monitor the solidification process of the frozen sand casting by measuring the temperature of the frozen sand mold during the pouring of molten metal; spray liquid nitrogen into the frozen sand mold during solidification to maintain the shape and integrity of the frozen sand mold; control the cooling rate of the casting by the amount of liquid nitrogen spray to achieve precise control of the solidification process of the casting, so that the casting can solidify layer by layer and improve the overall mechanical properties of the casting.

2. The method for cryogenic pressure regulation composite casting of a light alloy cabin for aerospace vehicles according to claim 1, characterized in that: The frozen sand mold is a multi-material frozen sand mold.

3. The method for cryogenic pressure regulation composite casting of a light alloy cabin for aerospace vehicles according to claim 1, characterized in that: Rapid cooling by spraying liquid nitrogen creates a temperature gradient from the end of the casting to the gate, enabling rapid solidification of the casting.

4. A cryogenic pressure-regulating composite casting forming system for aerospace vehicle lightweight alloy cabins according to any one of claims 1-3, characterized in that, The system comprises a cryogenic sand mold pressure regulating casting furnace and a cryogenic sand mold negative pressure regulating system. The cryogenic sand mold pressure regulating casting furnace includes an upper pressure cylinder (1-01) and a lower pressure cylinder (1-15). The upper pressure cylinder (1-01) is connected to the lower pressure cylinder (1-15) via a partition plate (1-10). The upper pressure cylinder (1-01) has a pressure signal acquisition hole (1-02) and an air inlet / outlet (1-03) on its side. A pressure relief valve (1-04) is located at the top of the upper pressure cylinder (1-01). The inner cavity of the upper pressure cylinder (1-01) is equipped with a cryogenic sand mold system (1-06) for a spacecraft cabin. Several cryogenic sand mold temperature sensors (1-07) are located within the cryogenic sand mold system (1-06). A crucible (1-18) is located inside the lower pressure cylinder (1-15). A plastic [material / material] is installed above the partition plate between the upper and lower cylinders. A separation membrane (1-21) is provided; a riser pipe (1-11) is provided in the partition plate, the lower end of the riser pipe (1-11) is inserted into the crucible (1-18) and a ceramic filter screen (1-12) is installed at the bottom; the upper end of the riser pipe (1-11) is connected to the cryogenic sand mold gate; a ceramic filter screen (1-08) is embedded in the cryogenic sand mold system (1-06) of the aerospace vehicle cabin; a liquid nitrogen cooling device (1-05) is provided around the cryogenic sand mold system (1-06) of the aerospace vehicle cabin; an electrode assembly (1-19) and a thermocouple assembly (1-20) are provided on the left side of the lower pressure cylinder (1-15) and a lower pressure cylinder pressure signal acquisition hole (1-13) and a lower pressure cylinder air inlet and outlet hole (1-14) are provided on the right side; a furnace lining (1-17) is connected to the outer wall of the crucible (1-18); a heating element (1-16) is provided in the furnace lining (1-17).

5. The cryogenic pressure-regulating composite casting forming system for a light alloy cabin of an aerospace vehicle according to claim 4, characterized in that, In the cryogenic sand mold negative pressure regulating system, the upper pressure cylinder inlet and outlet port (1-03) of the cryogenic sand mold regulating casting furnace (1) is connected to the vacuum buffer tank (5) in sequence through vacuum pressure gauge one (2), pneumatic ball valve one (3), and pneumatic ball valve two (4); the lower pressure cylinder inlet and outlet port (1-14) of the cryogenic sand mold regulating casting furnace (1) is connected to the gas storage tank (12) in sequence through vacuum pressure gauge two (8), digital combination valve two (9), pneumatic ball valve four (10), and pressure reducing valve (11); the liquid nitrogen storage tank (15) is connected to the liquid nitrogen connecting pipe at the upper end of the cryogenic sand mold regulating casting furnace (1) in sequence through digital combination valve two (14) and cryogenic sand mold temperature acquisition module (13); the cryogenic sand mold regulating casting furnace (1) is equipped with throttle valves (16) at the upper and lower ends.

Citation Information

Patent Citations

  • Precesion casting method for high temperature alloy complex thin-walled castings

    CN102699311A

  • Vacuum low-pressure casting forming device for titanium alloy component

    CN104028729A