Composition for preparing unburned bricks, unburned bricks and preparation method thereof
By using a combination of coal powder slag, ceramic waste slag, blast furnace slag and other raw materials with gypsum fiber and emulsified asphalt and other auxiliary materials, combined with anionic surfactants and polycarboxylic acid coagulants, the problem of insufficient strength and freeze-thaw resistance of unfired bricks is solved , achieving high strength and good freeze-thaw resistance.
Patent Information
- Application Number
- CN202410845939.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-06-27
AI Technical Summary
Existing unfired bricks have low strength and poor freeze-thaw resistance, and are easily cracked or damaged in cold areas due to expansion force caused by moisture freezing.
Using raw materials such as pulverized coal slag, ceramic waste slag, blast furnace slag, cement, emulsified asphalt, gypsum fiber, polycarboxylic acid coagulant, diisooctyl sebacate and anionic surfactant, it is prepared through a specific mixing and pressing process. Bricks, forming a gelling product to improve sealing and mechanical strength.
The strength and freeze-thaw resistance of the unfired bricks are significantly improved, the water absorption rate is reduced, the sealing and mechanical properties are enhanced, and the problem of insufficient freeze-thaw resistance is solved.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to a composition for preparing unburned bricks, unburned bricks and a preparation method thereof, and belongs to the technical field of solid waste recycling. Background Art
[0002] Unburned bricks are a new type of wall material, which are mainly made of fly ash, coal slag, coal gangue, tailings slag, chemical slag and other waste materials without high-temperature calcination. This type of unburned brick also realizes the resource utilization of industrial solid waste, solves pollution problems, saves soil resources and protects the environment. However, some existing unburned bricks also have some disadvantages: compared with traditional high-temperature fired bricks, the strength of unburned bricks is relatively low; in cold areas, when water freezes inside the bricks, it may generate expansion force, causing the bricks to crack or damage, and the freeze-thaw resistance of unburned bricks is relatively poor. Summary of the invention
[0003] In order to solve at least one problem existing in the above-mentioned prior art, the present invention provides a composition for preparing unfired bricks, unfired bricks and a preparation method thereof.
[0004] In order to achieve the above-mentioned purpose, the present invention adopts the following technical scheme: a composition for preparing unfired bricks, composed of the following raw materials and their weight parts: 25-30 parts of coal powder slag, 22-26 parts of ceramic waste slag, 13-17 parts of blast furnace slag, 10-13 parts of cement, 8-11 parts of emulsified asphalt, 2-4 parts of gypsum fiber, 2-4 parts of polycarboxylic acid coagulant, 1.5-3 parts of diisooctyl sebacate, 1-2 parts of anionic surfactant, and 4-7 parts of water; wherein the sum of the weight parts of coal powder slag, ceramic waste slag, blast furnace slag, cement, emulsified asphalt, gypsum fiber, polycarboxylic acid coagulant, diisooctyl sebacate, anionic surfactant and water is 100 parts.
[0005] Preferably, the composition for preparing unfired bricks is composed of the following raw materials and their weight parts: 28.5 parts of coal powder slag, 23.5 parts of ceramic waste slag, 14 parts of blast furnace slag, 11 parts of cement, 9 parts of emulsified asphalt, 2.8 parts of gypsum fiber, 3.1 parts of polycarboxylic acid coagulant, 2.1 parts of diisooctyl sebacate, 1.8 parts of anionic surfactant, and 4.5 parts of water.
[0006] Preferably, the particle sizes of coal powder slag, ceramic waste slag and blast furnace slag are all less than 1 mm.
[0007] Preferably, the length of the gypsum fibers is 1-2 mm.
[0008] Preferably, the anionic surfactant is one of alkyl sulfonate or alkylbenzene sulfonate.
[0009] Preferably, the anionic surfactant is one of sodium dodecyl sulfonate, sodium tetradecyl sulfonate, sodium hexadecyl sulfonate, sodium dodecylbenzene sulfonate or tetradecylbenzene sulfonate.
[0010] The composition of the unburned brick of the present invention is used for preparing the unburned brick.
[0011] The method for preparing unburned bricks of the present invention is to use the composition for preparing unburned bricks as raw materials and prepare the bricks by the following method:
[0012] (1) Firstly, crush the coal powder slag, ceramic waste slag and blast furnace slag to a particle size of less than 1 mm, mix them, then add cement, gypsum fiber and polycarboxylic acid coagulant, mix them evenly, and obtain mixed dry material;
[0013] (2) Mixing anionic surfactant, water, dioctyl sebacate and emulsified asphalt, and homogenizing at high speed to obtain a mixed emulsion;
[0014] (3) Add the mixed emulsion to the mixed dry material, homogenize and mix at a low speed to obtain grouting material;
[0015] (4) The grouting material is pressed into brick blanks and then cured to avoid firing the bricks.
[0016] Preferably, the rotation speed of the high-speed homogenizer is 2000-2500 rpm.
[0017] Preferably, the rotation speed of the low-speed homogenization is 100-150 rpm.
[0018] Preferably, the pressing pressure is 15-18 MPa.
[0019] Preferably, the curing conditions are: steam curing first, then natural curing, and then low-temperature curing.
[0020] Preferably, the steam curing temperature is 80-85° C. and the time is 40-60 min.
[0021] Preferably, the natural curing temperature is 30-35°C and the time is 10-12 days.
[0022] Preferably, the low temperature curing temperature is 10-15°C and the time is 12-16 hours.
[0023] Beneficial effects of the present invention: the composition for preparing unfired bricks of the present invention uses coal powder slag, ceramic waste slag, blast furnace slag, cement and emulsified asphalt as main ingredients, and uses gypsum fiber, anionic surfactant, diisooctyl sebacate and polycarboxylic acid coagulant as auxiliary ingredients, and is compounded in specific amounts. The prepared unfired bricks have higher strength and better anti-freezing and thawing effect. The composition for preparing unfired bricks of the present invention uses coal powder slag, ceramic waste slag and blast furnace slag as raw materials, recycles waste resources, solves ecological and environmental protection problems, and uses gypsum fiber and emulsified asphalt in synergy, so that the matrix of the unfired brick is more dense, which helps to improve the strength of the unfired bricks. degree; in addition, the composition for preparing unfired bricks of the present invention uses anionic surfactants, diethyl hexyl sebacate, and polycarboxylic acid coagulants to assist gypsum fibers, reduce the expansion of coal powder slag, ceramic waste slag, and blast furnace slag, enhance the solidification density of the composition, reduce the water absorption rate of the unfired bricks, and improve the strength and anti-freezing and thawing effect of the unfired bricks; the method for preparing unfired bricks of the present invention can secondary solidify the silicates of coal powder slag, ceramic waste slag, and blast furnace slag, and form a gelled product with the remaining components to bond together, have good sealing, make the unfired bricks have good hydrophobicity, and further improve the mechanical strength and unfired brick properties of the unfired bricks. DETAILED DESCRIPTION
[0024] The following is a clear and complete description of the technical solutions in the implementation of the present invention. The described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] A composition for preparing unfired bricks provided in an embodiment of the present invention is composed of the following raw materials and their weight parts: 25-30 parts of coal powder slag, 22-26 parts of ceramic waste slag, 13-17 parts of blast furnace slag, 10-13 parts of cement, 8-11 parts of emulsified asphalt, 2-4 parts of gypsum fiber, 2-4 parts of polycarboxylic acid coagulant, 1.5-3 parts of diisooctyl sebacate, 1-2 parts of anionic surfactant, and 4-7 parts of water; wherein the sum of the weight parts of coal powder slag, ceramic waste slag, blast furnace slag, cement, emulsified asphalt, gypsum fiber, polycarboxylic acid coagulant, diisooctyl sebacate, anionic surfactant and water is 100 parts; the particle sizes of coal powder slag, ceramic waste slag and blast furnace slag are all less than 1 mm; the length of gypsum fiber is 1-2 mm; the anionic surfactant is one of sodium dodecyl sulfonate, sodium tetradecyl sulfonate, sodium hexadecyl sulfonate, sodium dodecylbenzene sulfonate or tetradecylbenzene sulfonate.
[0026] The present invention also provides a method for preparing unburned bricks by using the composition for preparing unburned bricks as a raw material. The preparation method comprises the following steps:
[0027] (1) Firstly, crush the coal powder slag, ceramic waste slag and blast furnace slag to a particle size of less than 1 mm, mix them, then add cement, gypsum fiber and polycarboxylic acid coagulant, mix them evenly, and obtain mixed dry material;
[0028] (2) mixing anionic surfactant, water, dioctyl sebacate and emulsified asphalt, and homogenizing at a speed of 2000-2500 rpm to obtain a mixed emulsion;
[0029] (3) Add the mixed emulsion to the mixed dry material and perform low-speed homogenization mixing at a speed of 100-150 rpm to obtain grouting material;
[0030] (4) Place the grouting material in a mold and press it into a brick at a pressure of 15-18 MPa. Then steam cure it at a temperature of 80-85°C for 40-60 minutes, then naturally cure it at a temperature of 30-35°C for 10-12 days, and then low-temperature cure it at a temperature of 10-15°C for 12-16 hours to avoid burning the bricks.
[0031] Example 1
[0032] A composition for preparing unburned bricks, comprising the following raw materials and their weight parts, calculated based on 100 parts of the total weight of the raw materials: 25 parts of coal powder slag, 24.5 parts of ceramic waste slag, 17 parts of blast furnace slag, 13 parts of cement, 8 parts of emulsified asphalt, 2 parts of gypsum fibers with a length of 1 to 2 mm, 2 parts of polycarboxylic acid coagulant, 1.5 parts of diisooctyl sebacate, 1 part of sodium dodecylbenzene sulfonate, and 6 parts of water;
[0033] The steps of preparing unburned bricks are as follows:
[0034] (1) Firstly, crush the coal powder slag, ceramic waste slag and blast furnace slag to a particle size of less than 1 mm, mix them, then add cement, gypsum fiber and polycarboxylic acid coagulant, mix them evenly, and obtain mixed dry material;
[0035] (2) mixing anionic surfactant, water, dioctyl sebacate and emulsified asphalt, and homogenizing at a speed of 2000 rpm to obtain a mixed emulsion;
[0036] (3) Add the mixed emulsion to the mixed dry material and perform low-speed homogenization mixing at a speed of 150 rpm to obtain grouting material;
[0037] (4) Place the grouting material in a mold and press it into a brick at a pressure of 15 MPa. Then steam cure it at a temperature of 80-85°C for 50 minutes, then naturally cure it at a temperature of 30-35°C for 11 days, and then low-temperature cure it at a temperature of 10-15°C for 14 hours to avoid firing the bricks.
[0038] Example 2
[0039] A composition for preparing unburned bricks, composed of the following raw materials and their weight parts, calculated based on 100 parts of the total weight of the raw materials: 26 parts of coal powder slag, 26 parts of ceramic waste slag, 13 parts of blast furnace slag, 10 parts of cement, 10 parts of emulsified asphalt, 2.5 parts of gypsum fibers with a length of 1 to 2 mm, 3 parts of polycarboxylic acid coagulant, 2 parts of diisooctyl sebacate, 2 parts of sodium dodecylbenzene sulfonate, and 5.5 parts of water;
[0040] The steps of the method for preparing the unfired bricks in this embodiment 2 are exactly the same as those in embodiment 1.
[0041] Example 3
[0042] A composition for preparing unburned bricks, composed of the following raw materials and their weight parts, calculated based on 100 parts of the total weight of the raw materials: 28.5 parts of coal powder slag, 23.5 parts of ceramic waste slag, 14 parts of blast furnace slag, 11 parts of cement, 9 parts of emulsified asphalt, 2.8 parts of gypsum fibers with a length of 1 to 2 mm, 3.1 parts of polycarboxylic acid coagulant, 2.1 parts of diisooctyl sebacate, 1.8 parts of sodium dodecylbenzene sulfonate, and 4.5 parts of water;
[0043] The steps of the method for preparing the unfired bricks in this embodiment 3 are exactly the same as those in embodiment 1.
[0044] Example 4
[0045] A composition for preparing unburned bricks, composed of the following raw materials and their weight parts, calculated based on 100 parts of the total weight of the raw materials: 30 parts of coal powder slag, 22 parts of ceramic waste slag, 13 parts of blast furnace slag, 12 parts of cement, 8 parts of emulsified asphalt, 2 parts of gypsum fibers with a length of 1-2 mm, 3 parts of polycarboxylic acid coagulant, 2.5 parts of diisooctyl sebacate, 1.5 parts of sodium dodecylbenzene sulfonate, and 6 parts of water;
[0046] The steps for preparing the unfired bricks in this embodiment 4 are exactly the same as those in embodiment 1.
[0047] Example 5
[0048] A composition for preparing unburned bricks, comprising the following raw materials and their weight parts, calculated based on 100 parts of the total weight of the raw materials: 25 parts of coal powder slag, 22 parts of ceramic waste slag, 13 parts of blast furnace slag, 10.5 parts of cement, 9.5 parts of emulsified asphalt, 4 parts of gypsum fibers with a length of 1 to 2 mm, 4 parts of polycarboxylic acid coagulant, 3 parts of diisooctyl sebacate, 28 parts of sodium tetradecyl sulfonate, and 7 parts of water;
[0049] The steps for preparing the unfired bricks in this embodiment 5 are exactly the same as those in embodiment 1.
[0050] Example 6
[0051] A composition for preparing unburned bricks, comprising the following raw materials and their weight parts, calculated based on 100 parts of the total weight of the raw materials: 26.3 parts of coal powder slag, 25.2 parts of ceramic waste slag, 14.5 parts of blast furnace slag, 11 parts of cement, 9.3 parts of emulsified asphalt, 2.8 parts of gypsum fibers with a length of 1 to 2 mm, 2.5 parts of polycarboxylic acid coagulant, 2.6 parts of diisooctyl sebacate, 1.8 parts of sodium dodecyl sulfonate, and 4 parts of water;
[0052] The steps for preparing the unfired bricks in Example 6 are exactly the same as those in Example 1.
[0053] Example 7
[0054] A composition for preparing unburned bricks, composed of the following raw materials and their weight parts, calculated based on 100 parts of the total weight of the raw materials: 27.6 parts of coal powder slag, 22.8 parts of ceramic waste slag, 15.6 parts of blast furnace slag, 10.9 parts of cement, 8.5 parts of emulsified asphalt, 3.1 parts of gypsum fibers with a length of 1-2 mm, 2.8 parts of polycarboxylic acid coagulant, 2.1 parts of diisooctyl sebacate, 1.6 parts of sodium hexadecyl sulfonate, and 5 parts of water;
[0055] The steps for preparing the unfired bricks in this embodiment 7 are exactly the same as those in embodiment 1.
[0056] Example 8
[0057] A composition for preparing unburned bricks, composed of the following raw materials and their weight parts, calculated based on 100 parts of the total weight of the raw materials: 25 parts of coal powder slag, 24.5 parts of ceramic waste slag, 17 parts of blast furnace slag, 13 parts of cement, 8 parts of emulsified asphalt, 2 parts of gypsum fibers with a length of 1 to 2 mm, 2 parts of polycarboxylic acid coagulant, 1.5 parts of diisooctyl sebacate, 1 part of sodium tetradecylbenzene sulfonate, and 6 parts of water;
[0058] The steps of preparing unburned bricks are as follows:
[0059] (1) Firstly, crush the coal powder slag, ceramic waste slag and blast furnace slag to a particle size of less than 1 mm, mix them, then add cement, gypsum fiber and polycarboxylic acid coagulant, mix them evenly, and obtain mixed dry material;
[0060] (2) mixing anionic surfactant, water, dioctyl sebacate and emulsified asphalt, and homogenizing at a speed of 2500 rpm to obtain a mixed emulsion;
[0061] (3) Add the mixed emulsion to the mixed dry material and perform low-speed homogenization mixing at a speed of 100 rpm to obtain grouting material;
[0062] (4) Place the grouting material in a mold and press it into a brick at a pressure of 16 MPa. Then steam cure it at a temperature of 80-85°C for 40 minutes, then naturally cure it at a temperature of 30-35°C for 10 days, and then low-temperature cure it at a temperature of 10-15°C for 12 hours to avoid firing the bricks.
[0063] Example 9
[0064] A composition for preparing unburned bricks, composed of the following raw materials and their weight parts, calculated based on 100 parts of the total weight of the raw materials: 28.5 parts of coal powder slag, 23.5 parts of ceramic waste slag, 14 parts of blast furnace slag, 11 parts of cement, 9 parts of emulsified asphalt, 2.8 parts of gypsum fibers with a length of 1 to 2 mm, 3.1 parts of polycarboxylic acid coagulant, 2.1 parts of diisooctyl sebacate, 1.8 parts of sodium dodecyl sulfonate, and 4.5 parts of water;
[0065] The steps of preparing unburned bricks are as follows:
[0066] (1) Firstly, crush the coal powder slag, ceramic waste slag and blast furnace slag to a particle size of less than 1 mm, mix them, then add cement, gypsum fiber and polycarboxylic acid coagulant, mix them evenly, and obtain mixed dry material;
[0067] (2) mixing anionic surfactant, water, dioctyl sebacate and emulsified asphalt, and homogenizing at a speed of 2500 rpm to obtain a mixed emulsion;
[0068] (3) Add the mixed emulsion to the mixed dry material and perform low-speed homogenization mixing at a speed of 100 rpm to obtain grouting material;
[0069] (4) Place the grouting material in a mold and press it into a brick at a pressure of 18 MPa. Then steam cure it at a temperature of 80-85°C for 60 minutes, then naturally cure it at a temperature of 30-35°C for 12 days, and then low-temperature cure it at a temperature of 10-15°C for 16 hours to avoid firing the bricks.
[0070] Comparative Example 1
[0071] A composition for preparing unburned bricks, comprising the following raw materials and their weight parts, calculated based on 100 parts of the total weight of the raw materials: 25 parts of coal powder slag, 24.5 parts of ceramic waste slag, 17 parts of blast furnace slag, 13 parts of cement, 8 parts of emulsified asphalt, 2 parts of gypsum powder, 2 parts of polycarboxylic acid coagulant, 1.5 parts of diisooctyl sebacate, 1 part of sodium tetradecylbenzene sulfonate, and 6 parts of water; the gypsum powder replaces gypsum fibers with a length of 1 to 2 mm;
[0072] The steps for preparing the unfired bricks of Comparative Example 1 are exactly the same as those of Example 1.
[0073] Comparative Example 2
[0074] A composition for preparing unburned bricks, comprising the following raw materials and their weight parts, calculated based on 100 parts of the total weight of the raw materials: 26.5 parts of coal powder slag, 25 parts of ceramic waste slag, 17 parts of blast furnace slag, 13 parts of cement, 8 parts of emulsified asphalt, 2 parts of polycarboxylic acid coagulant, 1.5 parts of diisooctyl sebacate, 1 part of sodium tetradecylbenzene sulfonate, and 6 parts of water; excluding gypsum fibers with a length of 1 to 2 mm;
[0075] The steps for preparing the unfired bricks in Comparative Example 2 are exactly the same as those in Example 1.
[0076] Comparative Example 3
[0077] A composition for preparing unburned bricks is composed of the following raw materials and their weight parts, calculated based on 100 parts of the total weight of the raw materials: 30 parts of coal powder slag, 26 parts of ceramic waste slag, 17 parts of blast furnace slag, 13 parts of cement, 2 parts of gypsum fibers with a length of 1-2 mm, 2 parts of polycarboxylic acid coagulant, 3 parts of diisooctyl sebacate, 1 part of sodium tetradecylbenzene sulfonate, and 6 parts of water; and does not contain emulsified asphalt.
[0078] The steps for preparing the unfired bricks in Comparative Example 3 are exactly the same as those in Example 1.
[0079] Comparative Example 4
[0080] A composition for preparing unburned bricks, comprising the following raw materials and their weight parts, calculated based on 100 parts of the total weight of the raw materials: 25 parts of coal powder slag, 24.5 parts of ceramic waste slag, 17 parts of blast furnace slag, 13 parts of cement, 8 parts of emulsified asphalt, 2 parts of gypsum fibers with a length of 1 to 2 mm, 3.5 parts of polycarboxylic acid coagulant, 1 part of sodium tetradecylbenzene sulfonate, and 6 parts of water; and does not contain diisooctyl sebacate;
[0081] The steps for preparing the unfired bricks in Comparative Example 4 are exactly the same as those in Example 1.
[0082] Comparative Example 5
[0083] A composition for preparing unburned bricks, comprising the following raw materials and their weight parts, calculated based on 100 parts of the total weight of the raw materials: 25 parts of coal powder slag, 24.5 parts of ceramic waste slag, 17 parts of blast furnace slag, 13 parts of cement, 8 parts of emulsified asphalt, 2 parts of gypsum fibers with a length of 1 to 2 mm, 2 parts of polycarboxylic acid coagulant, 1.5 parts of diisooctyl sebacate, 1 part of sodium dodecylbenzene sulfonate, and 6 parts of water;
[0084] The steps of preparing unburned bricks are as follows:
[0085] (1) Firstly, crush the coal powder slag, ceramic waste slag and blast furnace slag to a particle size of less than 1 mm, mix them, then add cement, gypsum fiber and polycarboxylic acid coagulant, mix them evenly, and obtain mixed dry material;
[0086] (2) mixing anionic surfactant, water, dioctyl sebacate and emulsified asphalt, and homogenizing at a speed of 2500 rpm to obtain a mixed emulsion;
[0087] (3) Add the mixed emulsion to the mixed dry material and perform low-speed homogenization mixing at a speed of 100 rpm to obtain grouting material;
[0088] (4) Place the grouting material in a mold and press it into a brick at a pressure of 16 MPa. Then naturally cure it at a temperature of 30-35°C for 10 days, and then low-temperature cure it at a temperature of 10-15°C for 12 hours to avoid firing the bricks.
[0089] Comparative Example 6
[0090] A composition for preparing unburned bricks, comprising the following raw materials and their weight parts, calculated based on 100 parts of the total weight of the raw materials: 25 parts of coal powder slag, 24.5 parts of ceramic waste slag, 17 parts of blast furnace slag, 13 parts of cement, 8 parts of emulsified asphalt, 2 parts of gypsum fibers with a length of 1 to 2 mm, 2 parts of polycarboxylic acid coagulant, 1.5 parts of diisooctyl sebacate, 1 part of sodium dodecylbenzene sulfonate, and 6 parts of water;
[0091] The steps of preparing unburned bricks are as follows:
[0092] (1) Firstly, crush the coal powder slag, ceramic waste slag and blast furnace slag to a particle size of less than 1 mm, mix them, then add cement, gypsum fiber and polycarboxylic acid coagulant, mix them evenly, and obtain mixed dry material;
[0093] (2) mixing anionic surfactant, water, dioctyl sebacate and emulsified asphalt, and homogenizing at a speed of 2500 rpm to obtain a mixed emulsion;
[0094] (3) Add the mixed emulsion to the mixed dry material and perform low-speed homogenization mixing at a speed of 100 rpm to obtain grouting material;
[0095] (4) Place the grouting material in a mold and press it into a brick at a pressure of 16 MPa. Then naturally cure it at a temperature of 30-35°C for 10 days to avoid firing the bricks.
[0096] Comparative Example 7
[0097] A composition for preparing unburned bricks, comprising the following raw materials and their weight parts, calculated based on 100 parts of the total weight of the raw materials: 25 parts of coal powder slag, 24.5 parts of ceramic waste slag, 17 parts of blast furnace slag, 13 parts of cement, 8 parts of emulsified asphalt, 2 parts of gypsum fibers with a length of 1 to 2 mm, 2 parts of polycarboxylic acid coagulant, 1.5 parts of diisooctyl sebacate, 1 part of sodium dodecylbenzene sulfonate, and 6 parts of water;
[0098] The steps of preparing unburned bricks are as follows:
[0099] (1) Firstly, coal powder slag, ceramic waste slag and blast furnace slag are crushed to a particle size of less than 1 mm, mixed, and then cement, gypsum fiber, polycarboxylic acid coagulant, anionic surfactant, water, diisooctyl sebacate and emulsified asphalt are added, and high-speed homogenization is performed at a speed of 2500 rpm to obtain grouting material;
[0100] (2) Place the grouting material in a mold and press it into a brick at a pressure of 16 MPa. Then steam cure it at a temperature of 80-85°C for 40 minutes, then naturally cure it at a temperature of 30-35°C for 10 days, and then low-temperature cure it at a temperature of 10-15°C for 12 hours to avoid firing the bricks.
[0101] Effect embodiment:
[0102] The unfired bricks prepared in the above Examples 1 to 9 and Comparative Examples 1 to 7 were tested for density, compressive strength and freeze-thaw resistance according to GB / T2542-2012. The results are shown in Table 1.
[0103] Table 1
[0104]
[0105] From Table 1 above, the unfired bricks prepared by the present invention have higher density and excellent compressive strength. After 25 freeze-thaw cycles, the compressive strength loss rate and mass loss rate of the unfired bricks prepared by the present invention are relatively small, and have excellent anti-freeze and thaw performance.
[0106] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit and essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
[0107] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A composition for preparing unfired bricks, characterized in that: The invention is composed of the following raw materials, calculated based on the sum of 100 parts by weight: 25-30 parts of coal powder slag, 22-26 parts of ceramic waste slag, 13-17 parts of blast furnace slag, 10-13 parts of cement, 8-11 parts of emulsified asphalt, 2-4 parts of gypsum fiber, 2-4 parts of polycarboxylic acid coagulant, 1.5-3 parts of diisooctyl sebacate, 1-2 parts of anionic surfactant and 4-7 parts of water.
2. A composition for preparing unburned bricks according to claim 1, characterized in that: The composition is composed of the following raw materials, calculated by weight: 28.5 parts of coal powder slag, 23.5 parts of ceramic waste slag, 14 parts of blast furnace slag, 11 parts of cement, 9 parts of emulsified asphalt, 2.8 parts of gypsum fiber, 3.1 parts of polycarboxylic acid coagulant, 2.1 parts of diisooctyl sebacate, 1.8 parts of anionic surfactant, and 4.5 parts of water.
3. A composition for preparing unburned bricks according to claim 1, characterized in that: The particle sizes of the coal powder slag, ceramic waste slag and blast furnace slag are all less than 1 mm.
4. A composition for preparing unburned bricks according to claim 1, characterized in that: The length of the gypsum fiber is 1-2 mm.
5. A composition for preparing unburned bricks according to claim 1, characterized in that: The anionic surfactant is one of alkyl sulfonate or alkylbenzene sulfonate.
6. A composition for preparing unburned bricks according to claim 5, characterized in that: The anionic surfactant is one of sodium dodecyl sulfonate, sodium tetradecyl sulfonate, sodium hexadecyl sulfonate, sodium dodecylbenzene sulfonate or tetradecylbenzene sulfonate.
7. A non-fired brick, characterized in that: The unburned brick is prepared from the composition according to any one of claims 1 to 6.
8. A method for preparing unfired bricks, characterized in that: The method for preparing the unburned brick is carried out using the composition according to any one of claims 1 to 6, and the steps of the preparation method are as follows: (1) Firstly, crush the coal powder slag, ceramic waste slag and blast furnace slag to a particle size of less than 1 mm, mix them, then add cement, gypsum fiber and polycarboxylic acid coagulant, mix them evenly, and obtain a mixed dry material; (2) Mixing anionic surfactant, water, dioctyl sebacate and emulsified asphalt, and homogenizing at high speed to obtain a mixed emulsion; (3) Add the mixed emulsion to the mixed dry material, homogenize and mix at a low speed to obtain grouting material; (4) The grouting material is pressed into bricks, which are then first steam cured, then naturally cured, and finally low-temperature cured to avoid firing the bricks.
9. The method for preparing unburned bricks according to claim 8, characterized in that: The speed of high-speed homogenization in step (2) is 2000-2500 rpm; the speed of low-speed homogenization in step (3) is 100-150 rpm.
10. The method for preparing unburned bricks according to claim 8, characterized in that: The pressing pressure in step (4) is 15-18 MPa; the steam curing temperature is 80-85°C and the time is 40-60 min; the natural curing temperature is 30-35°C and the time is 10-12 d; the low-temperature curing temperature is 10-15°C and the time is 12-16 h.