A wear-resistant carbon fiber composite material and preparation method thereof
By introducing modified SiO2 nanoparticles and SiC nanowires into carbon fiber composite materials, combined with resin matrix and lubricant, the problem of difficulty in balancing performance in the existing technology is solved, and a wear-resistant carbon fiber composite material with excellent comprehensive properties is prepared, which is suitable for for many high-end applications.
Patent Information
- Application Number
- CN202410780414.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-06-18
AI Technical Summary
It is difficult for existing carbon fiber composite materials to take into account properties such as tensile strength when improving wear resistance, resulting in uneven performance.
A wear-resistant carbon fiber composite material composed of a resin matrix, modified carbon fiber, modified SiO2 nanoparticles, lubricants, antioxidants and compatibilizers is used to grow SiC nanowires in situ on chopped carbon fibers, and in the twin-screw Melt shearing, mixing, extrusion and granulation are carried out in the extruder to prepare materials with excellent impact properties, tensile properties, bending properties and wear resistance.
It has achieved an improvement in the comprehensive performance of the material, is suitable for many fields, and has excellent properties such as high strength and high modulus.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the field of carbon fiber composite materials, and in particular relates to a wear-resistant carbon fiber composite material and a preparation method thereof. Background Art
[0002] Carbon fiber is often used as a filler and compounded with resin, metal or ceramic substrates to improve the wear resistance of composite materials. It is widely used in high-end products in cutting-edge disciplines such as aerospace, electronics and electrical appliances, and can also be used in emerging fields such as drilling platforms, building materials and wind power generation. Although there are many types of carbon fiber composite materials, their performance varies. While improving wear resistance, it may ignore its tensile strength and other properties, making it difficult to take all properties into account. Summary of the invention
[0003] In view of this, the present invention aims to provide a wear-resistant carbon fiber composite material and a preparation method thereof to solve the above problems.
[0004] To achieve the above object, the technical solution of the present invention is achieved as follows:
[0005] A wear-resistant carbon fiber composite material, the composite material is prepared from raw materials including the following components:
[0006] Resin matrix 80-100 parts,
[0007] 5-15 parts of modified carbon fiber,
[0008] 3-5 parts of modified SiO2 nanoparticles,
[0009] Lubricant 0.5-3 parts,
[0010] 1-3 parts of antioxidant,
[0011] 2-4 parts of compatibilizer;
[0012] The resin matrix includes epoxy resin, nylon 66 and polyoxymethylene ultrafine powder in a weight ratio of (6-8): (3-5): (1-2).
[0013] Furthermore, the epoxy resin is bisphenol F epoxy resin, and the particle size of the polyoxymethylene ultrafine powder is 50nm-100nm.
[0014] Furthermore, the modified carbon fiber is SiC nanowires grown in situ on chopped carbon fibers, and the length of the chopped carbon fibers is 100-150 mm and the diameter is 10-20 μm.
[0015] Furthermore, the preparation method of the modified SiO2 nanoparticles is as follows: SiO2 nanoparticles and lanthanum oxide nanoparticles in a mass ratio of 1: (0.05-0.3) are sequentially added to a silane coupling agent and stirred evenly for later use.
[0016] Furthermore, the average particle size of the SiO2 nanoparticles is 10-15 nm, and the average particle size of the lanthanum oxide nanoparticles is 5-10 nm.
[0017] Furthermore, the lubricant is one or more of paraffin, silicone, and methyl silicone oil.
[0018] Furthermore, the antioxidant is a mixture of antioxidant AO-80 and antioxidant 618 in a weight ratio of (2-3):1.
[0019] Furthermore, the compatibilizer is maleic anhydride grafted polypropylene pp-g-MAH.
[0020] The present invention also provides a method for preparing the wear-resistant carbon fiber composite material as described above, the method comprising the following steps:
[0021] 1) In-situ growth of SiC nanowires on chopped carbon fibers to obtain modified carbon fibers;
[0022] 2) Add SiO2 nanoparticles and lanthanum oxide nanoparticles to the silane coupling agent in proportion and stir evenly to obtain modified SiO2 nanoparticles for use;
[0023] 3) Mix the resin matrix, lubricant, antioxidant and compatibilizer in proportion and stir evenly to obtain a mixture;
[0024] 4) Add the modified carbon fiber, modified SiO2 nanoparticles and the mixed material into a twin-screw extruder, and perform melt shearing, mixing and extrusion granulation at 260-330° C. in the twin-screw extruder to obtain a wear-resistant carbon fiber composite material.
[0025] Further, the specific steps of step 1) are:
[0026] 1.1) Soak the pretreated chopped carbon fibers in a 0.08 mol / L Ni(NO3)2 catalyst solution, then take them out and dry them for later use;
[0027] 1.2) Place the carbon fiber loaded with metal salt catalyst in a tubular furnace, use Si and SiO2 as silicon source and graphite as carbon source, and keep it warm in Ar atmosphere at 1150-1230℃ for 3-6h.
[0028] Compared with the prior art, the wear-resistant carbon fiber composite material and the preparation method thereof described in the present invention have the following advantages:
[0029] The wear-resistant carbon fiber composite material described in the present invention is prepared by combining raw materials such as a resin matrix, modified carbon fiber, and modified SiO2 nanoparticles. The wear-resistant carbon fiber composite material has good comprehensive performance, excellent impact resistance, tensile strength, bending resistance, and wear resistance, and can be applied to multiple fields. DETAILED DESCRIPTION
[0030] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments may be combined with each other.
[0031] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] Example 1
[0033] A wear-resistant carbon fiber composite material, the composite material is prepared from raw materials including the following components:
[0034] Resin matrix: 80 parts,
[0035] Modified carbon fiber: 5 parts,
[0036] Modified SiO2 nanoparticles: 3 parts,
[0037] Lubricant: 0.5 parts of silicone,
[0038] Antioxidant: 1 part, which is antioxidant AO-80 and 618 in a weight ratio of 2:1,
[0039] Compatibilizer: pp-g-MAH 2 parts;
[0040] The resin matrix includes bisphenol F epoxy resin, nylon 66 and polyoxymethylene ultrafine powder in a weight ratio of 6:3:1, and the particle size of the polyoxymethylene ultrafine powder is 50nm.
[0041] The method for preparing the above-mentioned wear-resistant carbon fiber composite material comprises the following steps:
[0042] 1) In-situ growth of SiC nanowires on chopped carbon fibers
[0043] 1.1) Pretreatment of chopped carbon fiber
[0044] The chopped carbon fibers were ultrasonically degreased in acetone for 15 minutes, then rinsed with deionized water and anhydrous ethanol in sequence and dried at 200°C for 1 hour; the chopped carbon fibers were then immersed in a NaOH solution for 10 minutes to remove surface impurities, then rinsed with deionized water three times and dried at 200°C for 2 hours;
[0045] 1.2) Soak the pretreated chopped carbon fibers in a 0.08 mol / L Ni(NO3)2 catalyst solution for 3 h, then take them out and dry them at 80°C for 5 h for later use;
[0046] 1.3) The carbon fiber loaded with the catalyst was placed in a tubular furnace, with Si and SiO2 as silicon sources and graphite as carbon source, and kept warm for 6 hours in an Ar atmosphere at 1225°C, with the mass ratio of SiO2, Si and graphite being 1:0.3:0.5, and the flow rate of Ar being 150 mL / min, and the temperature was increased to 1230°C at a heating rate of 5°C / min, and kept warm at this temperature for 6 hours, and then the heating was stopped and cooled to room temperature with the furnace, and the modified carbon fiber was obtained by opening the furnace;
[0047] 2) SiO2 nanoparticles and lanthanum oxide nanoparticles in a mass ratio of 1:0.1 are sequentially added to the silane coupling agent KH550 and stirred evenly to obtain modified SiO2 nanoparticles for standby use. The mass ratio of SiO2 nanoparticles to the silane coupling agent is 1:20;
[0048] 3) Mix the resin matrix, lubricant, antioxidant and compatibilizer in proportion and stir evenly to obtain a mixture;
[0049] 4) Add the modified carbon fiber, modified SiO2 nanoparticles and the mixed material into a twin-screw extruder, and obtain the wear-resistant carbon fiber composite material through melt shearing, mixing and extrusion granulation. The temperature of each zone of the twin-screw extruder is as follows: the temperature of the front section of the barrel is 290°C; the middle section is 300°C; the rear section is 310°C; and the nozzle is 310°C.
[0050] The properties of the obtained wear-resistant carbon fiber composite material are shown in Table 1.
[0051] Example 2
[0052] A wear-resistant carbon fiber composite material, the composite material is prepared from raw materials including the following components:
[0053] Resin matrix: 95 parts,
[0054] Modified carbon fiber: 8 parts,
[0055] Modified SiO2 nanoparticles: 5 parts,
[0056] Lubricant: 2.5 parts of silicone,
[0057] Antioxidant: 2 parts, antioxidant AO-80 and 618 in a weight ratio of 3:1,
[0058] Compatibilizer: pp-g-MAH 3.5 parts;
[0059] The resin matrix includes bisphenol F epoxy resin, nylon 66 and polyoxymethylene ultrafine powder in a weight ratio of 7:3:1, and the particle size of the polyoxymethylene ultrafine powder is 65nm.
[0060] The method for preparing the above-mentioned wear-resistant carbon fiber composite material comprises the following steps:
[0061] 1) In-situ growth of SiC nanowires on chopped carbon fibers
[0062] 1.1) Pretreatment of chopped carbon fiber
[0063] The chopped carbon fibers were ultrasonically degreased in acetone for 15 minutes, then rinsed with deionized water and anhydrous ethanol in sequence and dried at 200°C for 1 hour; the chopped carbon fibers were then immersed in a NaOH solution for 10 minutes to remove surface impurities, then rinsed with deionized water three times and dried at 200°C for 2 hours;
[0064] 1.2) Soak the pretreated chopped carbon fibers in a 0.08 mol / L Ni(NO3)2 catalyst solution for 3 h, then take them out and dry them at 80°C for 5 h for later use;
[0065] 1.3) The carbon fiber loaded with the catalyst was placed in a tubular furnace, with Si and SiO2 as silicon sources and graphite as carbon source, and kept warm for 6 hours in an Ar atmosphere at 1225°C, with the mass ratio of SiO2, Si and graphite being 1:0.3:0.5, and the flow rate of Ar being 150 mL / min, and the temperature was increased to 1230°C at a heating rate of 5°C / min, and kept warm at this temperature for 6 hours, and then the heating was stopped and cooled to room temperature with the furnace, and the modified carbon fiber was obtained by opening the furnace;
[0066] 2) SiO2 nanoparticles and lanthanum oxide nanoparticles in a mass ratio of 1:0.15 are sequentially added to the silane coupling agent KH550 and stirred evenly to obtain modified SiO2 nanoparticles for standby use. The mass ratio of SiO2 nanoparticles to the silane coupling agent is 1:20;
[0067] 3) Mix the resin matrix, lubricant, antioxidant and compatibilizer in proportion and stir evenly to obtain a mixture;
[0068] 4) Add the modified carbon fiber, modified SiO2 nanoparticles and the mixed material into a twin-screw extruder, and obtain the wear-resistant carbon fiber composite material through melt shearing, mixing and extrusion granulation. The temperature of each zone of the twin-screw extruder is as follows: the temperature of the front section of the barrel is 290°C; the middle section is 300°C; the rear section is 310°C; and the nozzle is 310°C.
[0069] The properties of the obtained wear-resistant carbon fiber composite material are shown in Table 1.
[0070] Example 3
[0071] A wear-resistant carbon fiber composite material, the composite material is prepared from raw materials including the following components:
[0072] Resin matrix: 100 parts,
[0073] Modified carbon fiber: 10 parts,
[0074] Modified SiO2 nanoparticles: 5 parts,
[0075] Lubricant: 3 parts, silicone and paraffin in a weight ratio of 1:1,
[0076] Antioxidant: 3 parts, antioxidant AO-80 and 618 with a weight ratio of 2.6:1,
[0077] Compatibilizer: pp-g-MAH 4 parts;
[0078] The resin matrix includes bisphenol F epoxy resin, nylon 66 and polyoxymethylene ultrafine powder in a weight ratio of 8:5:1.5, and the particle size of the polyoxymethylene ultrafine powder is 80nm.
[0079] The method for preparing the above-mentioned wear-resistant carbon fiber composite material comprises the following steps:
[0080] 1) In-situ growth of SiC nanowires on chopped carbon fibers
[0081] 1.1) Pretreatment of chopped carbon fiber
[0082] The chopped carbon fibers were ultrasonically degreased in acetone for 15 minutes, then rinsed with deionized water and anhydrous ethanol in sequence and dried at 200°C for 1 hour; the chopped carbon fibers were then immersed in a NaOH solution for 10 minutes to remove surface impurities, then rinsed with deionized water three times and dried at 200°C for 2 hours;
[0083] 1.2) Soak the pretreated chopped carbon fibers in a 0.08 mol / L Ni(NO3)2 catalyst solution for 3 h, then take them out and dry them at 80°C for 5 h for later use;
[0084] 1.3) The carbon fiber loaded with the catalyst was placed in a tubular furnace, with Si and SiO2 as silicon sources and graphite as carbon source, and kept warm for 6 hours in an Ar atmosphere at 1225°C, with the mass ratio of SiO2, Si and graphite being 1:0.3:0.5, and the flow rate of Ar being 150 mL / min, and the temperature was increased to 1230°C at a heating rate of 5°C / min, and kept warm at this temperature for 6 hours, and then the heating was stopped and cooled to room temperature with the furnace, and the modified carbon fiber was obtained by opening the furnace;
[0085] 2) SiO2 nanoparticles and lanthanum oxide nanoparticles in a mass ratio of 1:0.2 are sequentially added to the silane coupling agent KH550 and stirred evenly to obtain modified SiO2 nanoparticles for standby use, and the mass ratio of SiO2 nanoparticles to the silane coupling agent is 1:20;
[0086] 3) Mix the resin matrix, lubricant, antioxidant and compatibilizer in proportion and stir evenly to obtain a mixture;
[0087] 4) Add the modified carbon fiber, modified SiO2 nanoparticles and the mixed material into a twin-screw extruder, and obtain the wear-resistant carbon fiber composite material through melt shearing, mixing and extrusion granulation. The temperature of each zone of the twin-screw extruder is as follows: the temperature of the front section of the barrel is 290°C; the middle section is 300°C; the rear section is 310°C; and the nozzle is 310°C.
[0088] The properties of the obtained wear-resistant carbon fiber composite material are shown in Table 1.
[0089] Comparative Example 1
[0090] The difference from Example 3 is that the resin matrix only uses bisphenol F epoxy resin.
[0091] Comparative Example 2
[0092] The difference from Example 3 is that no polyoxymethylene ultrafine powder is added to the resin matrix.
[0093] Comparative Example 3
[0094] The difference from Example 3 is that the weight ratio of bisphenol F epoxy resin, nylon 66 and polyoxymethylene ultrafine powder is 1:1:1.
[0095] Comparative Example 4
[0096] The difference from Example 3 is that the particle size of polyoxymethylene is 100 μm.
[0097] Comparative Example 5
[0098] The difference from Example 3 is that the carbon fibers are not modified.
[0099] Comparative Example 6
[0100] The difference from Example 3 is that SiC nanowires are prepared according to the same raw material ratio, and then the SiC nanowires are mixed with chopped carbon fibers to prepare a composite material.
[0101] Comparative Example 7
[0102] The difference from Example 3 is that the SiO2 nanoparticles are not doped with lanthanum oxide nanoparticles.
[0103] Comparative Example 8
[0104] The difference from Example 3 is that the mass ratio of SiO2 nanoparticles to lanthanum oxide nanoparticles is 1:1.
[0105] Table 1 Performance comparison of each embodiment and each comparative example
[0106]
[0107] It can be seen from the above table that the wear-resistant carbon fiber composite material prepared in the embodiment of the present invention has good comprehensive performance, not only is it wear-resistant, but also has excellent properties such as high strength and high modulus.
[0108] By comparing Example 3 with Comparative Examples 1-4, it can be found that the resin matrix plays an important role in the formulation of the present invention. The lack of a certain matrix, the change of the proportion of the resin matrix, and the particle size will affect the various properties of the material. Polyoxymethylene is a linear polymer with no side chain, high density, and high crystallinity, and has excellent comprehensive properties. Using it as an auxiliary matrix can effectively increase the overall performance of the resin matrix. At the same time, the polyoxymethylene ultrafine powder not only makes the polyoxymethylene more evenly dispersed, but also helps to improve the mechanical properties and wear resistance of the material.
[0109] By comparing Example 3 and Comparative Examples 5-6, it can be found that carbon fiber modified with SiC nanowires is more conducive to improving the overall performance of the material, and the effect of simply mixing SiC nanowires and carbon fibers is not very obvious, and it is more beneficial to grow SiC nanowires on carbon fibers as a whole.
[0110] By comparing Example 3 and Comparative Examples 7-8, it can be found that doping with a small amount of lanthanum oxide nanoparticles can improve the mechanical properties and wear resistance of the material, and if the content of lanthanum oxide nanoparticles increases, it is not conducive to improving the material properties.
[0111] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A wear-resistant carbon fiber composite material, characterized in that: The composite material is prepared from raw materials including the following components: Resin matrix 80-100 parts, 5-15 parts of modified carbon fiber, 3-5 parts of modified SiO2 nanoparticles, Lubricant 0.5-3 parts, 1-3 parts of antioxidant, 2-4 parts of compatibilizer; The resin matrix comprises epoxy resin, nylon 66 and polyoxymethylene ultrafine powder in a weight ratio of (6-8): (3-5): (1-2); The epoxy resin is bisphenol F type epoxy resin, and the particle size of the polyoxymethylene ultrafine powder is 50nm-100nm; The modified carbon fiber is SiC nanowire grown in situ on chopped carbon fiber, and the length of the chopped carbon fiber is 100-150 mm and the diameter is 10-20 μm; The preparation method of the modified SiO2 nanoparticles is as follows: SiO2 nanoparticles and lanthanum oxide nanoparticles with a mass ratio of 1: (0.05-0.3) are sequentially added into a silane coupling agent and stirred evenly for later use; The lubricant is silicone or silicone and paraffin in a weight ratio of 1:1; The average particle size of SiO2 nanoparticles is 10-15nm, and the average particle size of lanthanum oxide nanoparticles is 5-10nm.
2. The wear-resistant carbon fiber composite material according to claim 1, characterized in that: The antioxidant is a mixture of antioxidant AO-80 and antioxidant 618 in a weight ratio of (2-3):
1.
3. The wear-resistant carbon fiber composite material according to claim 1, characterized in that: The compatibilizer is maleic anhydride grafted polypropylene pp-g-MAH.
4. A method for preparing a wear-resistant carbon fiber composite material according to any one of claims 1 to 3, characterized in that: The method comprises the following steps: 1) In-situ growth of SiC nanowires on chopped carbon fibers to obtain modified carbon fibers; 2) Add SiO2 nanoparticles and lanthanum oxide nanoparticles to the silane coupling agent in proportion and stir evenly to obtain modified SiO2 nanoparticles for use; 3) Mix the resin matrix, lubricant, antioxidant and compatibilizer in proportion and stir evenly to obtain a mixture; 4) Add the modified carbon fiber, modified SiO2 nanoparticles and the mixed material into a twin-screw extruder, and perform melt shearing, mixing and extrusion granulation at 260-330° C. in the twin-screw extruder to obtain a wear-resistant carbon fiber composite material.
5. The method for preparing the wear-resistant carbon fiber composite material according to claim 4, characterized in that: The specific steps of step 1) are: 1.1) Soak the pretreated chopped carbon fibers in a 0.08 mol / L Ni(NO3)2 catalyst solution, then take them out and dry them for later use; 1.2) Place the carbon fiber loaded with metal salt catalyst in a tubular furnace, using Si and SiO2 as silicon source and graphite as carbon source, and keep it warm in an Ar atmosphere at 1150-1230℃ for 3-6h.
Citation Information
Patent Citations
Carbon fiber cloth surface oriented SiC nanowire array and preparation method thereof
CN115058885A
Anti-aging glass fiber reinforced plastic composite material and preparation method thereof