A method for recovering palladium from spent palladium-carbon catalyst

Through the roasting and alkaline thiocyanate + amino acid method oxygen pressure synergistic leaching of palladium in the autoclave, the high cost and low efficiency problems of palladium recovery from failed palladium carbon catalysts were solved, and efficient palladium recovery and low environmental pollution were achieved, improving ensure production continuity and economic benefits.

CN118389843BActive Publication Date: 2024-10-11XUZHOU GUOMAO VALUABLE & RARE METAL COMPREHENSIVE UTILIZATION INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410830941.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-11
Estimated Expiration
2044-06-26

AI Technical Summary

Technical Problem

The existing methods for recovering palladium from failed palladium carbon catalysts have problems of high cost, low efficiency and environmental pollution. In particular, the palladium leaching process requires high concentrations of thiocyanate and strong oxidants, resulting in low metal recovery rates and Production is discontinuous and personnel efficiency is low.

Method used

The method of roasting and heat preservation pretreatment and alkaline thiocyanate + amino acid method oxygen pressure synergistic leaching in palladium in the autoclave is used to replace the traditional reduction pretreatment and washing process through the synergistic effect of high temperature decomposition of hydrazine hydrate and iron oxide to improve metal recovery. rate and production continuity, and control the potential through oxygen pressure to improve the leaching rate of palladium.

Benefits of technology

Efficient recovery of palladium is achieved, with a leaching rate of more than 99%. The grade of precious metals contained in the slag is reduced, and the SCN-loss rate is reduced to less than 20%. This reduces wastewater generation and operation time, and improves production efficiency and economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118389843B_ABST
    Figure CN118389843B_ABST
Patent Text Reader

Abstract

The present application provides a method for recovering palladium in an invalid palladium carbon catalyst, comprising the following steps: step (A) calcining and heat-insulating the invalid palladium carbon catalyst for pretreatment; step (B) after the heat preservation in step (A) is completed, taking out the calcined invalid palladium carbon catalyst and ball milling it to obtain an invalid palladium carbon catalyst powder with a particle size of 50-200 mesh; step (C) putting the invalid palladium carbon catalyst powder obtained in step (B) into an autoclave, preparing a liquid-solid ratio of 3-5, adjusting the pH to 10-14, and then introducing them into the autoclave together and slurry mixing, covering the autoclave and evacuating the gas, starting stirring and heating to 50-60 degrees, and heat-insulating for 1-3 hours; step (D) after the heat preservation in step (C) is completed, continuing to heat the autoclave to 70-90°C, and heat-insulating for 1-3 hours. The present application has a reasonable structure, combines the fact that iron oxide is an alkaline oxide that does not react under alkaline conditions and the high-temperature reaction decomposition characteristics of hydrazine hydrate and iron oxide, improves metal recovery rate, continuous production, simple operation, and improved production efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to a method for recovering precious metal palladium, and specifically, to a method for recovering palladium from a spent palladium-carbon catalyst. Background Art

[0002] Palladium has the advantage of high catalytic activity and is widely used in the petroleum catalysis industry, automobile exhaust catalysts, pharmaceutical catalysts, etc. During use, palladium catalysts will lose their activity due to poisoning, carbon deposition, changes in carrier structure, metal grain aggregation or loss, etc., and need to be replaced regularly. The medical industry alone uses about 5,000 tons of palladium-carbon catalysts, and the waste catalysts that need to be replaced each year contain about 10 tons of palladium, which has high economic value. Therefore, vigorously developing a circular economy and recovering platinum group metals from waste catalysts are of great significance in the fields of economic development, scientific research, and environmental protection, and their economic benefits are also very objective.

[0003] In the prior art, the thiocyanate method is an efficient and environmentally friendly palladium leaching method with broad application prospects. The thiocyanate palladium leaching system is mainly composed of thiocyanate and an oxidant. Depending on the leaching environment and the properties of the raw materials, the oxidant is usually Fe 3+ 、MnO 2 , O 2 , H 2 O 2 et al., SCN in the process of palladium leaching by thiocyanate method − It has a strong ability to form complexes with Pd(II) and Pd(IV), and the palladium leaching rate is close to that of the traditional aqua regia dissolution method; it has good selectivity, but the concentration of thiocyanate required in the palladium leaching process is high, and there will be thiocyanate in the residual liquid, which is costly and limits the large-scale industrial application of thiocyanate leaching.

[0004] In the glycine method, glycine is a non-toxic, non-volatile reagent with low production cost. Within a wide range of pH, Eh and temperature, due to the deprotonation of the amino acid group, glycine and palladium can form a stable complex with certain palladium-dissolving properties, but the palladium-dissolving rate is slow during the palladium leaching process under room temperature conditions.

[0005] In the method for recovering palladium from spent palladium-carbon catalysts, due to the influence of residual reducing agent after reduction pretreatment of palladium-containing waste before leaching on the palladium leaching process, the raw materials need to be rinsed with water after the reduction is completed, generating a large amount of wastewater, and the washing process causes the palladium metal attached to the surface of the waste to be lost with the washing water, resulting in a reduced metal recovery rate, a long washing process, inability to continuously produce, low personnel efficiency, and increased enterprise costs. Therefore, a method for recovering palladium from spent palladium-carbon catalysts is urgently needed to solve the above-mentioned problems. Summary of the invention

[0006] In view of the shortcomings of the prior art, the purpose of the present application is to provide a method for recovering palladium from an expired palladium-carbon catalyst to solve the problems raised in the above-mentioned background technology.

[0007] In order to achieve the above object, the present application provides a method for recovering palladium from an spent palladium-carbon catalyst, characterized in that it comprises the following steps:

[0008] Step (A) pre-treating the spent palladium-carbon catalyst by calcination and heat preservation;

[0009] Step (B) After the heat preservation in step (A) is completed, the spent palladium carbon catalyst after calcination is taken out and ball milled to obtain spent palladium carbon catalyst powder with a particle size of 50-200 mesh;

[0010] Step (C) putting the spent palladium carbon catalyst powder obtained in step (B) into an autoclave, preparing a liquid-solid ratio of 3-5, adjusting the pH to 10-14, and then introducing them into the autoclave together and slurrying, covering the autoclave and venting the gas, starting stirring and heating to 50-60 degrees, and keeping warm for 1-3 hours;

[0011] The liquid is: a thiocyanate solution with a concentration of 0.5-1.5 mol / L, and the amount of hydrazine hydrate added is 0.5%-1%;

[0012] Among them, the solids are: amino acid content is 1%-3%, and the iron oxide addition amount is 1%-2%;

[0013] Step (D) After the insulation in step (C) is completed, continue to heat the autoclave to 70-90°C and keep it warm for 1-3 hours;

[0014] Step (E) After the insulation in step (D) is completed, the autoclave is further heated to 120-140°C, oxygen is passed through to maintain the oxygen pressure at 1.2-2 MPa, and the insulation is performed for 8-12 hours;

[0015] Step (F) Step (E) After the heat preservation reaction is completed, stop heating and oxygen supply, and cool down with cooling water. When the temperature inside the autoclave drops to 20-40°C, open the exhaust valve to release gas. After the gas in the autoclave is completely released, take out the product in the autoclave and filter and wash it;

[0016] Step (G) subjecting the filtrate obtained in step (F) to resin adsorption and resin analysis to obtain a palladium-containing filtrate, and recovering palladium;

[0017] Step (H) The tailings after filtering and washing in step (F) are tested for palladium grade, and the filtrate after resin adsorption in step (G) is tested for SCN - concentration;

[0018] Step (I) Detection of SCN in Step (H) -concentration, add 10%-30% of the original amount of thiocyanate added in step (C), and repeat steps (C) to (H) for subsequent cyclic leaching.

[0019] Preferably, the thiocyanate solution in step (C) comprises one or more of a sodium thiocyanate solution and an ammonium thiocyanate solution.

[0020] Preferably, the amino acids in step (C) include one or more of glycine, alanine, histidine, and aspartic acid.

[0021] Preferably, the calcination pretreatment temperature in step (A) is 500-700° C. and the temperature is maintained for 3-6 hours.

[0022] Preferably, in step (B), the ball milling obtains spent palladium-carbon catalyst powder with a particle size of 200 meshes.

[0023] Preferably, in step (C), the liquid-to-solid ratio is prepared to be 5, the pH is adjusted to 12, the mixture is stirred and heated to 60 degrees, and kept warm for 2 hours.

[0024] Preferably, in step (D), the autoclave is heated to 60° C. and kept warm for 2 hours.

[0025] Preferably, in step (E), the autoclave is further heated to 140° C., oxygen is passed through to maintain an oxygen pressure of 1.2 MPa, and the temperature is maintained for 12 hours.

[0026] According to a method for recovering palladium from an expired palladium carbon catalyst of the present application, by combining the fact that iron oxide is an alkaline oxide and does not react under alkaline conditions and the high-temperature reaction and decomposition characteristics of hydrazine hydrate and iron oxide, the reduction pretreatment-high-temperature decomposition process of the expired palladium carbon catalyst after roasting replaces the original reduction pretreatment-washing process, without generating excess waste water and without metal loss in the washing process with washing water, thereby improving metal recovery rate, continuous production, simple operation, and improved production efficiency;

[0027] After hydrazine hydrate is decomposed at high temperature, the temperature is raised, and the alkaline thiocyanate method + amino acid method oxygen pressure synergistic palladium leaching method is adopted. The oxygen pressure increases the active potential of oxygen. Compared with the traditional method of adding strong oxidants, it is easier to control the potential for palladium leaching. The palladium leaching rate reaches more than 99%, and the precious metal grade of slag is reduced to less than 50g / t. At the same time, thiocyanate and amino acid synergistically leaching palladium, SCN - The loss rate is reduced to less than 20%, achieving efficient palladium leaching. Compared with the traditional method, if a high palladium leaching rate is to be maintained under normal pressure, a strong oxidant needs to be added. SCN - If the loss rate is greater than 50%, the production cost will increase;

[0028] The alkaline thiocyanate + amino acid method of oxygen pressure leaching palladium is adopted. The temperature is increased to increase the complexation rate of thiocyanate and amino acid with palladium ions and reduce the palladium leaching time. Compared with the traditional process, the leaching time is reduced by 4-8h while maintaining a high leaching rate. At the same time, the solution has high purity, does not introduce new impurity ions, is green and pollution-free, and is conducive to subsequent cyclic palladium leaching. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Other features, objects and advantages of the present application will become more apparent by reading the detailed description of non-limiting embodiments with reference to the following drawings:

[0030] Figure 1 The present invention is a flow chart of a method for recovering palladium from a spent palladium-carbon catalyst according to one embodiment of the present application. DETAILED DESCRIPTION

[0031] In order to make the technical means, creative features, objectives and effects achieved by this application easy to understand, this application is further explained below in conjunction with specific implementation methods.

[0032] like Figure 1 As shown, the present application provides a technical solution: a method for recovering palladium from an expired palladium-carbon catalyst, comprising the following steps:

[0033] Step (A) pre-treating the spent palladium-carbon catalyst by calcination and heat preservation;

[0034] Step (B) After the heat preservation in step (A) is completed, the spent palladium carbon catalyst after calcination is taken out and ball milled to obtain spent palladium carbon catalyst powder with a particle size of 50-200 mesh;

[0035] Step (C) putting the spent palladium carbon catalyst powder obtained in step (B) into an autoclave, preparing a liquid-solid ratio of 3-5, adjusting the pH to 10-14, and then introducing them into the autoclave together and slurrying, covering the autoclave and venting the gas, starting stirring and heating to 50-60 degrees, and keeping warm for 1-3 hours;

[0036] The liquid is: a thiocyanate solution with a concentration of 0.5-1.5 mol / L, and the amount of hydrazine hydrate added is 0.5%-1%;

[0037] Among them, the solid is: the amino acid content is 1%-3%, and the iron oxide addition amount is 1%-2%. This design is convenient for the reduction pretreatment of the failed palladium carbon catalyst after roasting;

[0038] Step (D): After the heat preservation in step (C) is completed, the autoclave is continued to be heated to 70-90°C and kept warm for 1-3 hours. After the reduction is completed, this design combines the fact that iron oxide is an alkaline oxide that does not react under alkaline conditions and the high-temperature reaction and decomposition characteristics of hydrazine hydrate and iron oxide. This process is a high-temperature decomposition of hydrazine hydrate, which reduces the impact of residual hydrazine hydrate on the subsequent leaching process. Unlike the traditional reduction leaching process in which water rinsing is added after the reduction is completed, this process is continuously operated by adjusting the temperature;

[0039] Step (E) After the insulation in step (D) is completed, the autoclave is further heated to 120-140°C, oxygen is passed through to maintain the oxygen pressure at 1.2-2MPa, and the temperature is maintained for 8-12 hours. This design begins to use the alkaline thiocyanate method + amino acid method to synergistically oxygen pressure leaching palladium on the failed palladium carbon catalyst. In this process, oxygen is passed through to maintain a certain oxygen pressure, control the potential, maintain a high leaching rate, reduce the reaction time, and reduce the SCN - Decomposition, without adding new strong oxidants, reduces the complexation of impurity ions such as iron, copper and other metal ions with amino acids in the system, forms substances that are more stable than palladium thiocyanate complex and palladium amino acid complex, and reduces the loss of thiocyanate and amino acids;

[0040] Step (F) Step (E) After the heat preservation reaction is completed, stop heating and oxygen supply, and cool down with cooling water. When the temperature inside the autoclave drops to 20-40°C, open the exhaust valve to release gas. After the gas in the autoclave is completely released, take out the product in the autoclave and filter and wash it;

[0041] Step (G) The filtrate obtained in step (F) is subjected to resin adsorption and resin analysis to obtain a palladium-containing filtrate, and palladium is recovered. This design and process does not introduce new impurities, is green and pollution-free, and is conducive to the subsequent recycling of tail liquid for palladium leaching process;

[0042] Step (H) The tailings after filtering and washing in step (F) are tested for palladium grade, and the filtrate after resin adsorption in step (G) is tested for SCN - concentration;

[0043] Step (I) Detection of SCN in Step (H) - concentration, adding 10%-30% of the original amount of thiocyanate added in step (C), wherein the added amount is solid thiocyanate, and repeating steps (C) to step (H) for subsequent cyclic leaching.

[0044] Preferably, the thiocyanate solution in step (C) comprises one or more of a sodium thiocyanate solution and an ammonium thiocyanate solution.

[0045] Preferably, the amino acids in step (C) include one or more of glycine, alanine, histidine, and aspartic acid.

[0046] Preferably, the calcination pretreatment temperature in step (A) is 500-700° C. and the temperature is maintained for 3-6 hours.

[0047] Preferably, in step (B), the ball milling obtains spent palladium-carbon catalyst powder with a particle size of 200 meshes.

[0048] Preferably, in step (C), the liquid-to-solid ratio is prepared to be 5, the pH is adjusted to 12, the mixture is stirred and heated to 60 degrees, and kept warm for 2 hours.

[0049] Preferably, in step (D), the autoclave is heated to 60° C. and kept warm for 2 hours.

[0050] Preferably, in step (E), the autoclave is further heated to 140° C., oxygen is passed through to maintain an oxygen pressure of 1.2 MPa, and the temperature is maintained for 12 hours.

[0051] A specific embodiment is described below according to a method for recovering palladium from a spent palladium-carbon catalyst of the present invention.

[0052] Example 1: Step (A1) calcining and pre-treating the spent palladium-carbon catalyst, wherein the calcination temperature is 700° C. and the temperature is kept for 3 hours;

[0053] Step (B1): After the heat preservation in step (A1) is completed, the spent palladium carbon catalyst after calcination is taken out and ball milled to obtain spent palladium carbon catalyst powder with a particle size of 200 mesh;

[0054] Step (C1) 100 g of the spent palladium carbon catalyst powder obtained in step (B1) is put into an autoclave, a sodium thiocyanate solution with a liquid-to-solid ratio of 5 and a concentration of 1 mol / L is prepared, 1% glycine is added, 0.6% hydrazine hydrate is added, and 2% iron oxide is added, and the pH is adjusted to 13, and then introduced into the autoclave together and slurry is adjusted, the autoclave is covered and the gas is evacuated, stirring is turned on, heating to 60 degrees, and keeping warm for 3 hours;

[0055] Step (D1) After the heat preservation in step (C1) is completed, the autoclave is continued to be heated to 70°C and kept warm for 3 hours;

[0056] Step (E1): After the heat preservation in step (D1) is completed, the autoclave is further heated to 120°C, oxygen is passed through to maintain the oxygen pressure at 1.2 MPa, and the heat preservation is performed for 12 hours;

[0057] Step (F1) Step (E1) After the heat preservation reaction is completed, stop heating and oxygen supply, and cool down with cooling water. When the temperature inside the autoclave drops to 30°C, open the exhaust valve to release gas. After the gas in the autoclave is completely released, take out the product in the autoclave and filter and wash it;

[0058] Step (G1) subjecting the filtrate obtained in step (F1) to resin adsorption and resin analysis to obtain a palladium-containing filtrate, and recovering palladium;

[0059] The grade of the spent palladium carbon catalyst after calcination in step (H1) is 4123 g / t. The tailings after filtration and washing in step (F1) are weighed to 83.35 g and the palladium grade is 49 g / t. The palladium leaching rate is 99.01%. At the same time, the filtrate after resin adsorption in step (G1) is tested for SCN - The concentration is 0.81 mol / L;

[0060] Step (I1) Detection of SCN in step (H1) - The concentration is 0.81 mol / L, 19% of the original amount of sodium thiocyanate added in step (C1) is added, and steps (C1) to (H1) are repeated for subsequent cyclic leaching.

[0061] Example 2: Step (A2) calcining and pre-treating the spent palladium-carbon catalyst, wherein the calcination temperature is 500° C. and the temperature is kept for 6 hours;

[0062] Step (B2): After the heat preservation in step (A2) is completed, the spent palladium carbon catalyst after calcination is taken out and ball milled to obtain spent palladium carbon catalyst powder with a particle size of 200 mesh;

[0063] Step (C2) 100 g of the spent palladium carbon catalyst powder obtained in step (B2) is put into an autoclave, a sodium thiocyanate solution with a liquid-to-solid ratio of 5 and a concentration of 1 mol / L is prepared, 3% alanine is added, 1% hydrazine hydrate is added, and 2% iron oxide is added, and the pH is adjusted to 13, and then introduced into the autoclave together and slurry is adjusted, the autoclave is covered and the gas is evacuated, stirring is turned on, heating to 60 degrees, and keeping warm for 2 hours;

[0064] Step (D2): After the heat preservation in step (C2) is completed, the autoclave is continued to be heated to 70°C and kept warm for 3 hours;

[0065] Step (E2): After the heat preservation in step (D2) is completed, the autoclave is further heated to 140°C, oxygen is passed through to maintain the oxygen pressure at 2 MPa, and the heat preservation is performed for 12 hours;

[0066] Step (F2) Step (E2) After the heat preservation reaction is completed, stop heating and oxygen supply, and cool down with cooling water. When the temperature inside the autoclave drops to 30°C, open the exhaust valve to release gas. After the gas in the autoclave is completely released, take out the product in the autoclave and filter and wash it;

[0067] Step (G2) subjecting the filtrate obtained in step (F2) to resin adsorption and resin analysis to obtain a palladium-containing filtrate, and recovering palladium;

[0068] The grade of the spent palladium carbon catalyst after calcination in step (H2) is 4123 g / t. The tailings after filtration and washing in step (F2) are weighed to 81.35 g and the palladium grade is 43 g / t. The palladium leaching rate is 99.15%. At the same time, the filtrate after resin adsorption in step (G2) is tested for SCN - The concentration is 0.84 mol / L;

[0069] Step (I2) Detection of SCN in step (H2) - The concentration is 0.84 mol / L, 16% of the original amount of sodium thiocyanate added in step (C2) is added, and steps (C2) to (H2) are repeated for subsequent cyclic leaching.

[0070] Example 3: Step (A3) The spent palladium carbon catalyst is subjected to a calcination and heat preservation pretreatment, wherein the calcination temperature is 700° C. and the heat preservation is 3 hours;

[0071] Step (B3) After the heat preservation in step (A3) is completed, the spent palladium carbon catalyst after calcination is taken out and ball milled to obtain spent palladium carbon catalyst powder with a particle size of 200 mesh;

[0072] Step (C3) 100 g of the spent palladium carbon catalyst powder obtained in step (B3) is put into an autoclave, a liquid-to-solid ratio of 5 and a concentration of 1 mol / L ammonium thiocyanate solution are prepared, 2% glycine is added, 0.5% hydrazine hydrate is added, and 2% iron oxide is added, and the pH is adjusted to 12, and then introduced into the autoclave together and slurry is adjusted, the autoclave is covered and the gas is evacuated, stirring is turned on, heating to 60 degrees, and keeping warm for 2 hours;

[0073] Step (D3) After the heat preservation in step (C3) is completed, the autoclave is continued to be heated to 60°C and kept warm for 2 hours;

[0074] Step (E3) After the insulation in step (D3) is completed, the autoclave is further heated to 140°C, oxygen is passed through to maintain the oxygen pressure at 1.2 MPa, and the insulation is continued for 12 hours;

[0075] Step (F3) Step (E3) After the heat preservation reaction is completed, stop heating and oxygen supply, and cool down with cooling water. When the temperature inside the autoclave drops to 30°C, open the exhaust valve to release gas. After the gas in the autoclave is completely released, take out the product in the autoclave and filter and wash it;

[0076] Step (G3) subjecting the filtrate obtained in step (F3) to resin adsorption and resin analysis to obtain a palladium-containing filtrate, and recovering palladium;

[0077] The grade of the spent palladium carbon catalyst after calcination in step (H3) is 4123 g / t. The tailings after filtration and washing in step (F3) are weighed to 82.88 g and the palladium grade is 42 g / t. The palladium leaching rate is 99.16%. At the same time, the filtrate after resin adsorption in step (G3) is tested for SCN - The concentration is 0.82 mol / L;

[0078] Step (I3) SCN detected in step (H3) - The concentration is 0.82 mol / L, 18% of the original amount of ammonium thiocyanate added in step (C3) is added, and steps (C3) to (H3) are repeated for subsequent cyclic leaching.

[0079] According to Examples 1-3, by combining the fact that iron oxide is an alkaline oxide that does not react under alkaline conditions and the high-temperature reaction and decomposition characteristics of hydrazine hydrate and iron oxide, the reduction pretreatment-high-temperature decomposition process of the depleted palladium carbon catalyst after roasting replaces the original reduction pretreatment-washing process, without generating excess waste water, and without metal loss during the washing process with the washing water, the metal recovery rate is improved, the production is continuous, the operation is simple, and the production efficiency is improved;

[0080] After hydrazine hydrate is decomposed at high temperature, the temperature is raised, and the alkaline thiocyanate method + amino acid method oxygen pressure synergistic palladium leaching method is adopted. The oxygen pressure increases the active potential of oxygen. Compared with the traditional method of adding strong oxidants, it is easier to control the potential for palladium leaching. The palladium leaching rate reaches more than 99%, and the precious metal grade of slag is reduced to less than 50g / t. At the same time, thiocyanate and amino acid synergistically leaching palladium, SCN - The loss rate is reduced to less than 20%, achieving efficient palladium leaching. Compared with the traditional method, which maintains a high palladium leaching rate under normal pressure, it is necessary to add a strong oxidant, SCN - The loss rate is greater than 50%;

[0081] The alkaline thiocyanate + amino acid method of oxygen pressure leaching palladium is adopted. The temperature is increased to increase the complexation rate of thiocyanate and amino acid with palladium ions and reduce the palladium leaching time. Compared with the traditional process, the leaching time is reduced by 4-8h while maintaining a high leaching rate. At the same time, the solution has high purity, does not introduce new impurity ions, is green and pollution-free, and is conducive to subsequent cyclic palladium leaching.

[0082] The present invention discloses a method for recovering palladium from an invalid palladium-carbon catalyst, which combines the advantages and disadvantages of the thiocyanate method and the glycine method to carry out coordinated palladium leaching. The alkaline thiocyanate + glycine coordinated leaching system is used. Under pressurized conditions, oxygen is passed through to maintain a certain oxygen pressure, thereby increasing the oxygen potential of oxygen in the reactor, better controlling the potential, maintaining a high leaching rate, and reducing the decomposition of thiocyanate. No other strong oxidants are added during the leaching process, thereby reducing the influence of impurity ions such as Fe, Cu, and Mn on the palladium leaching process. At the same time, the temperature is increased to increase the glycine palladium leaching rate, thereby further reducing the loss of thiocyanate.

[0083] The combination of alkaline thiocyanate + glycine, the reduction pretreatment of the failed palladium carbon catalyst - hydrazine hydrate decomposition - leaching process realizes short-process continuous and efficient operation, overcoming the problems of large amount of washing water, metal loss, discontinuous operation, low work efficiency, serious environmental pollution in the leaching process, unstable palladium leaching rate, etc. in the traditional process of palladium pretreatment and washing process. While maintaining a high palladium leaching rate, it shortens the production cycle, reduces costs and increases efficiency, reduces operating difficulty, increases the palladium leaching rate, and improves production efficiency.

[0084] The above shows and describes the basic principles, main features and advantages of the present invention. It should be understood by those skilled in the art that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for recovering palladium from an expired palladium-carbon catalyst, characterized in that: The following steps are involved: Step (A) pre-treating the spent palladium-carbon catalyst by calcination and heat preservation; Step (B) After the heat preservation in step (A) is completed, the spent palladium carbon catalyst after calcination is taken out and ball milled to obtain spent palladium carbon catalyst powder with a particle size of 50-200 mesh; Step (C) putting the spent palladium carbon catalyst powder obtained in step (B) into an autoclave, preparing a liquid-solid ratio of 3-5, adjusting the pH to 10-14, and then introducing them into the autoclave together and slurrying, covering the autoclave and venting the gas, starting stirring and heating to 50-60 degrees, and keeping warm for 1-3 hours; The liquid is: a thiocyanate solution with a concentration of 0.5-1.5 mol / L, and the amount of hydrazine hydrate added is 0.5%-1%; Among them, the solids are: amino acid content is 1%-3%, and the iron oxide addition amount is 1%-2%; Step (D) After the insulation in step (C) is completed, continue to heat the autoclave to 70-90°C and keep it warm for 1-3 hours; Step (E) After the insulation in step (D) is completed, the autoclave is further heated to 120-140°C, oxygen is passed through to maintain the oxygen pressure at 1.2-2 MPa, and the insulation is performed for 8-12 hours; Step (F) Step (E) After the heat preservation reaction is completed, stop heating and oxygen supply, and cool down with cooling water. When the temperature inside the autoclave drops to 20-40°C, open the exhaust valve to release gas. After the gas in the autoclave is completely released, take out the product in the autoclave and filter and wash it; Step (G) subjecting the filtrate obtained in step (F) to resin adsorption and resin analysis to obtain a palladium-containing filtrate, and recovering palladium; Step (H) The tailings after filtering and washing in step (F) are tested for palladium grade, and the filtrate after resin adsorption in step (G) is tested for SCN - concentration; Step (I) Detection of SCN in Step (H) - concentration, add 10%-30% of the original amount of thiocyanate added in step (C), and repeat steps (C) to (H) for subsequent cyclic leaching.

2. A method for recovering palladium from a spent palladium-carbon catalyst according to claim 1, characterized in that: The thiocyanate solution in step (C) includes one or more of a sodium thiocyanate solution and an ammonium thiocyanate solution.

3. A method for recovering palladium from a spent palladium-carbon catalyst according to claim 1, characterized in that: The amino acids in step (C) include one or more of glycine, alanine, histidine, and aspartic acid.

4. A method for recovering palladium from a spent palladium-carbon catalyst according to claim 1, characterized in that: The temperature of the calcination pretreatment in the step (A) is 500-700° C. and the temperature is kept for 3-6 hours.

5. A method for recovering palladium from a spent palladium-carbon catalyst according to claim 1, characterized in that: In the step (B), the spent palladium-carbon catalyst powder with a particle size of 200 mesh is obtained by ball milling.

6. The method for recovering palladium from a spent palladium-carbon catalyst according to claim 1, characterized in that: In the step (C), the liquid-to-solid ratio is prepared to be 5, the pH is adjusted to 12, stirred and heated to 60 degrees, and kept warm for 2 hours.

7. The method for recovering palladium from a spent palladium-carbon catalyst according to claim 1, characterized in that: In the step (D), the autoclave is heated to 60° C. and kept warm for 2 hours.

8. The method for recovering palladium from a spent palladium-carbon catalyst according to claim 1, characterized in that: In the step (E), the autoclave is further heated to 140° C., oxygen is passed through the autoclave to maintain an oxygen pressure of 1.2 MPa, and the temperature is maintained for 12 hours.