Preparation method and application of viscose fiber containing camellia seed oil
By modifying viscose fiber with modified polyamide and graphene oxide, combined with camellia seed oil, the problem of insufficient strength and easy combustion of existing viscose fiber is solved, and excellent flame retardant, antibacterial and tensile properties are achieved. Suitable for the production of diaper materials.
Patent Information
- Application Number
- CN202410840490.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-06-27
AI Technical Summary
The existing viscose fiber has low strength, is easy to burn, and has insufficient flame retardant properties, antibacterial properties and tensile strength, which limits its application scope.
Using a preparation method containing camellia seed oil, through the modification of modified polyamide, graphene oxide and viscose fiber, azelaic acid, p-phenylenediamine, 3,5-dibromophenol, flake graphite, 4- Chemical substances such as aminophenol undergo multi-step reactions and treatments to form fibers with excellent flame retardant, antibacterial and tensile properties.
It improves the flame retardant, antibacterial and tensile properties of viscose fiber, enhances the anti-inflammatory effect of the fiber, is suitable for the production of children's and adult diaper materials, and improves the safety and comfort of the product.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of viscose fibers, in particular to a preparation method and application of viscose fibers containing camellia seed oil. Background Art
[0002] Viscose fiber is a cellulose fiber extracted and reshaped from natural lignin. It has the characteristics of being smooth, cool, breathable, antistatic, and UV-resistant. It is widely used in various underwear, textiles, clothing, non-woven and other fields. Existing viscose fibers are prepared by the most basic process and have low strength. Since wood fibers are easy to burn, many accidents will occur in actual use, and the application field will be limited. Therefore, improving the flame retardant properties, antibacterial properties, and tensile strength of viscose fibers can effectively improve the strength of viscose fibers and expand their application range. Summary of the invention
[0003] 1. Technical issues to be resolved
[0004] In view of the deficiencies in the prior art, the present invention provides a preparation method and application of viscose fiber containing camellia seed oil, which has excellent flame retardant, antibacterial and anti-inflammatory, and tensile properties.
[0005] (II) Technical solution
[0006] A method for preparing viscose fiber containing camellia seed oil is as follows:
[0007] a. Heat azelaic acid to a molten state under pressure, add p-phenylenediamine, stir and react for 2-6 hours, reduce the pressure to atmospheric pressure at 1MPa / h to obtain molten polyamide; add 3,5-dibromophenol to the methanol solution, stir and dissolve, heat to 50-60°C, add molten polyamide thereto, add initiator ammonium persulfate, heat to 80-120°C, react for 3-8 hours, stop the reaction, and cool to room temperature to obtain modified polyamide;
[0008] b. The modified polyamide is mixed with the viscose stock solution, camellia oil is added, heated to 100-150°C, stirred and mixed, then cooled to room temperature, filtered, and the filtrate is defoamed with a defoaming agent to obtain a modified viscose fiber primary stock solution;
[0009] c. In an ice-water mixture, add flake graphite to concentrated sulfuric acid, slowly add potassium permanganate while stirring, store at a temperature below 5°C for 50-100 h, then add it to deionized water, stir and react at a temperature below 35°C for 1-5 h, heat to 90-100°C and react for 1-3 h, then add 30% hydrogen peroxide and let stand for 10-20 h, wash with 5% hydrochloric acid and deionized water, and dry to obtain graphene oxide;
[0010] d. Add 4-aminophenol to water, stir evenly, add 2,3-epoxypropyltrimethylammonium chloride and sodium hydroxide, heat to 100-150°C, and stir continuously for 1-5 h to obtain 4-aminophenol grafted quaternary ammonium salt; add graphene oxide to dimethylformamide, stir evenly, and ultrasonically treat for 1-2 h to obtain a graphene oxide suspension, then add 4-aminophenol grafted quaternary ammonium salt and dicyclohexylcarbocyanide, ultrasonically treat for 5-10 min, react at 120-150°C for 30-60 h, add anhydrous ethanol and let stand overnight, remove the upper clear night, filter the lower precipitate with a polytetrafluoroethylene membrane, wash with ethanol and deionized water, and dry to obtain modified graphene oxide;
[0011] e. Add the modified viscose fiber primary stock solution into a high-pressure reactor, add modified graphene oxide, seal it, react at 140-180°C for 10-20 h, take it out and wash it with 60-80°C distilled water for 3-6 times, dry it to constant weight, and spin it into long and thin fibers on a spinning machine. After water cooling, pulling, spinning, acid coagulation, stretching, curing with a curing agent, washing, and drying processes, viscose fibers containing camellia seed oil are obtained.
[0012] Preferably, in step a, the mass ratio of azelaic acid, p-phenylenediamine, 3,5-dibromophenol and initiator ammonium persulfate is 1:0.8~1.2:0.3~0.6:0.01~0.03.
[0013] Preferably, in step b, the mass ratio of the modified polyamide, viscose stock solution and camellia oil is 1:10-30:1-15.
[0014] Preferably, the defoaming agent in step b is one of emulsified silicone oil, polyoxyethylene polyoxypropylene pentaerythritol ether, and polyoxyethylene polyoxypropanolamine ether.
[0015] Preferably, in step c, the mass ratio of flake graphite, concentrated sulfuric acid, potassium permanganate and hydrogen peroxide is 1:10~25:2~5:1.5~3.
[0016] Preferably, in step d, the mass ratio of 4-aminophenol, 2,3-epoxypropyltrimethylammonium chloride, sodium hydroxide and dicyclohexylcarbocyanine is 1:0.6~1.2:0.05~0.1:0.2~0.6.
[0017] Preferably, in step e, the mass ratio of the modified viscose fiber primary solution to the modified graphene oxide is 1:0.05-0.3.
[0018] Preferably, the viscose fiber containing camellia seed oil obtained by the method for preparing viscose fiber containing camellia seed oil is used in diaper materials.
[0019] 3. Beneficial technical effects
[0020] A viscose fiber containing camellia seed oil is prepared by modifying viscose fiber with modified polyamide and modified graphene oxide and adding camellia seed oil. The modified polyamide is 3,5-dibromophenol modified polyamide, and the modified graphene oxide is 4-aminophenol grafted quaternary ammonium salt 2,3-epoxypropyltrimethylammonium chloride. Halogen bromine has excellent flame retardant properties, polyamide can improve the tensile properties of the fiber, quaternary ammonium salt can improve the antibacterial property, and camellia seed oil can improve the antibacterial and anti-inflammatory effects.
[0021] The viscose fiber of the invention has excellent flame retardant, antibacterial and tensile properties, is comfortable to the body, easy to absorb, has good anti-inflammatory effect, and is suitable for the production of diaper materials for children and adults. DETAILED DESCRIPTION
[0022] Example 1
[0023] a. Under pressure, heat 10 g of azelaic acid to a molten state, add 8 g of p-phenylenediamine, stir and react for 2 h, reduce the pressure to atmospheric pressure at 1 MPa / h to obtain molten polyamide; add 3 g of 3,5-dibromophenol to 30 mL of methanol solution, stir and dissolve, heat to 50°C, add molten polyamide thereto, add 0.1 g of initiator ammonium persulfate, heat to 80°C, react for 3 h, stop the reaction, and cool to room temperature to obtain modified polyamide.
[0024] b. Mix 10 g of modified polyamide with 100 g of viscose stock solution, add 10 g of camellia oil, heat to 100 ° C and stir to mix, then cool to room temperature, filter, and defoam the filtrate with a defoaming agent emulsified silicone oil to obtain a modified viscose fiber primary stock solution.
[0025] c. In an ice-water mixture, add 10 g of flake graphite to 100 mL of concentrated sulfuric acid, slowly add 20 g of potassium permanganate while stirring, keep the mixture at a temperature below 5°C for 50 h, then add it to 400 mL of deionized water, stir and react at a temperature below 35°C for 1 h, heat to 90°C and react for 1 h, then add 20 mL of 30% hydrogen peroxide and let stand for 10 h, wash with 5% hydrochloric acid and deionized water, and dry to obtain graphene oxide.
[0026] d. Add 20 g of 4-aminophenol to 150 mL of water, stir evenly, add 12 g of 2,3-epoxypropyltrimethylammonium chloride and 1 g of sodium hydroxide, heat to 100°C, and stir continuously for 1 h to obtain 4-aminophenol grafted quaternary ammonium salt; add graphene oxide to 200 mL of dimethylformamide, stir evenly, and ultrasonically treat for 1 h to obtain a graphene oxide suspension, then add 4-aminophenol grafted quaternary ammonium salt and 4 g of dicyclohexylcarbocyanine, ultrasonically treat for 5 min, react at 120°C for 30 h, add anhydrous ethanol and let stand overnight, remove the upper clear night, filter the lower precipitate with a polytetrafluoroethylene membrane, wash with ethanol and deionized water, and dry to obtain modified graphene oxide.
[0027] e. Add 20 g of modified viscose fiber primary stock solution into a high-pressure reactor, add 1 g of modified graphene oxide, seal it, react at 140°C for 10 h, take it out and wash it three times with 60°C distilled water, dry it to constant weight, and spin it into long and thin fibers on a spinning machine. After water cooling, pulling, spinning, acid coagulation, stretching, curing with a curing agent, washing, and drying processes, viscose fibers containing camellia seed oil are obtained.
[0028] Example 2
[0029] a. Under pressure, heat 30 g of azelaic acid to a molten state, add 36 g of p-phenylenediamine, stir and react for 6 h, reduce the pressure to atmospheric pressure at 1 MPa / h to obtain molten polyamide; add 18 g of 3,5-dibromophenol to 120 mL of methanol solution, stir and dissolve, heat to 60°C, add molten polyamide thereto, add 0.3 g of initiator ammonium persulfate, heat to 120°C, react for 8 h, stop the reaction, and cool to room temperature to obtain modified polyamide.
[0030] b. 50 g of modified polyamide was mixed with 1500 g of viscose stock solution, 150 g of camellia oil was added, heated to 150 ℃ and stirred, then cooled to room temperature, filtered, and the filtrate was defoamed with a defoaming agent polyoxyethylene polyoxypropylene pentaerythritol ether to obtain a modified viscose fiber primary stock solution.
[0031] c. In an ice-water mixture, add 30 g of flake graphite to 350 mL of concentrated sulfuric acid, slowly add 150 g of potassium permanganate while stirring, keep the temperature below 5°C for 100 h, then add it to 1200 mL of deionized water, stir and react at below 35°C for 5 h, heat to 100°C and react for 3 h, then add 60 mL of 30% hydrogen peroxide and let stand for 20 h, wash with 5% hydrochloric acid and deionized water, and dry to obtain graphene oxide.
[0032] d. Add 60 g of 4-aminophenol to 800 mL of water, stir evenly, add 72 g of 2,3-epoxypropyltrimethylammonium chloride and 6 g of sodium hydroxide, heat to 150°C, and stir continuously for 5 h to obtain 4-aminophenol grafted quaternary ammonium salt; add graphene oxide to 600 mL of dimethylformamide, stir evenly, and ultrasonically treat for 2 h to obtain a graphene oxide suspension, then add 4-aminophenol grafted quaternary ammonium salt and 36 g of dicyclohexylcarbocyanine, ultrasonically treat for 10 min, react at 150°C for 60 h, add anhydrous ethanol and let stand overnight, remove the upper clear night, filter the lower precipitate with a polytetrafluoroethylene membrane, wash with ethanol and deionized water, and dry to obtain modified graphene oxide.
[0033] e. Add 60 g of modified viscose fiber primary stock solution into a high-pressure reactor, add 18 g of modified graphene oxide, seal it, react at 180°C for 20 h, take it out and wash it 6 times with 80°C distilled water, dry it to constant weight, and spin it into long and thin fibers on a spinning machine. After water cooling, pulling, spinning, acid coagulation, stretching, curing with a curing agent, washing, and drying processes, viscose fibers containing camellia seed oil are obtained.
[0034] Example 3
[0035] a. Under pressure, heat 15 g of azelaic acid to a molten state, add 15 g of p-phenylenediamine, stir and react for 3 h, reduce the pressure to atmospheric pressure at 1 MPa / h to obtain molten polyamide; add 8 g of 3,5-dibromophenol to 50 mL of methanol solution, stir and dissolve, heat to 55°C, add molten polyamide thereto, add 0.2 g of initiator ammonium persulfate, heat to 90°C, react for 5 h, stop the reaction, and cool to room temperature to obtain modified polyamide.
[0036] b. 20 g of modified polyamide was mixed with 300 g of viscose stock solution, 50 g of camellia oil was added, heated to 120 ° C and stirred, then cooled to room temperature, filtered, and the filtrate was defoamed with a defoaming agent polyoxyethylene polyoxypropanolamine ether to obtain a modified viscose fiber primary stock solution.
[0037] c. In an ice-water mixture, add 15 g of flake graphite to 200 mL of concentrated sulfuric acid, slowly add 50 g of potassium permanganate while stirring, keep the temperature below 5°C for 60 h, then add it to 600 mL of deionized water, stir and react at below 35°C for 2 h, heat to 92°C and react for 2 h, then add 40 mL of 30% hydrogen peroxide and let stand for 12 h, wash with 5% hydrochloric acid and deionized water, and dry to obtain graphene oxide.
[0038] d. Add 30 g of 4-aminophenol to 300 mL of water, stir evenly, add 30 g of 2,3-epoxypropyltrimethylammonium chloride and 3 g of sodium hydroxide, heat to 120°C, and stir continuously for 3 h to obtain 4-aminophenol grafted quaternary ammonium salt; add graphene oxide to 300 mL of dimethylformamide, stir evenly, and ultrasonically treat for 2 h to obtain a graphene oxide suspension, then add 4-aminophenol grafted quaternary ammonium salt and 16 g of dicyclohexylcarbocyanine, ultrasonically treat for 5 min, react at 130°C for 40 h, add anhydrous ethanol and let stand overnight, remove the upper clear night, filter the lower precipitate with a polytetrafluoroethylene membrane, wash with ethanol and deionized water, and dry to obtain modified graphene oxide.
[0039] e. Add 30 g of modified viscose fiber primary stock solution into a high-pressure reactor, add 5 g of modified graphene oxide, seal it, react at 150°C for 12 h, take it out and wash it with 65°C distilled water for 5 times, dry it to constant weight, and spin it into long and thin fibers on a spinning machine. After water cooling, pulling, spinning, acid coagulation, stretching, curing with a curing agent, washing, and drying processes, viscose fibers containing camellia seed oil are obtained.
[0040] Example 4
[0041] a. Under pressure, heat 20 g of azelaic acid to a molten state, add 20 g of p-phenylenediamine, stir and react for 4 h, reduce the pressure to atmospheric pressure at 1 MPa / h to obtain molten polyamide; add 10 g of 3,5-dibromophenol to 80 mL of methanol solution, stir and dissolve, heat to 58°C, add molten polyamide thereto, add 0.2 g of initiator ammonium persulfate, heat to 100°C, react for 6 h, stop the reaction, and cool to room temperature to obtain modified polyamide.
[0042] b. 30 g of modified polyamide was mixed with 800 g of viscose stock solution, 100 g of camellia oil was added, heated to 130 ° C and stirred, then cooled to room temperature, filtered, and the filtrate was defoamed with a defoaming agent emulsified silicone oil to obtain a modified viscose fiber primary stock solution.
[0043] c. In an ice-water mixture, add 25 g of flake graphite to 300 mL of concentrated sulfuric acid, slowly add 100 g of potassium permanganate while stirring, and store at a temperature below 5°C for 80 h. Then add it to 800 mL of deionized water, stir and react at a temperature below 35°C for 2 h, heat to 100°C and react for 3 h, then add 60 mL of 30% hydrogen peroxide and let stand for 18 h. Wash with 5% hydrochloric acid and deionized water, and dry to obtain graphene oxide.
[0044] d. Add 40 g of 4-aminophenol to 600 mL of water, stir evenly, add 45 g of 2,3-epoxypropyltrimethylammonium chloride and 3 g of sodium hydroxide, heat to 140°C, and stir continuously for 4 h to obtain 4-aminophenol grafted quaternary ammonium salt; add graphene oxide to 500 mL of dimethylformamide, stir evenly, and ultrasonically treat for 1 h to obtain a graphene oxide suspension, then add 4-aminophenol grafted quaternary ammonium salt and 20 g of dicyclohexylcarbocyanine, ultrasonically treat for 10 min, react at 150°C for 50 h, add anhydrous ethanol and let stand overnight, remove the upper clear night, filter the lower precipitate with a polytetrafluoroethylene membrane, wash with ethanol and deionized water, and dry to obtain modified graphene oxide.
[0045] e. Add 40 g of modified viscose fiber primary stock solution into a high-pressure reactor, add 12 g of modified graphene oxide, seal it, react at 160°C for 15 h, take it out and wash it 5 times with 70°C distilled water, dry it to constant weight, and spin it into long and thin fibers on a spinning machine. After water cooling, pulling, spinning, acid coagulation, stretching, curing with a curing agent, washing, and drying processes, viscose fibers containing camellia seed oil are obtained.
[0046] Example 5
[0047] a. Under pressure, heat 28 g of azelaic acid to a molten state, add 32 g of p-phenylenediamine, stir and react for 5 h, reduce the pressure to atmospheric pressure at 1 MPa / h to obtain molten polyamide; add 15 g of 3,5-dibromophenol to 100 mL of methanol solution, stir and dissolve, heat to 58°C, add molten polyamide thereto, add 0.3 g of initiator ammonium persulfate, heat to 110°C, react for 6 h, stop the reaction, and cool to room temperature to obtain modified polyamide.
[0048] b. 40 g of modified polyamide was mixed with 1200 g of viscose stock solution, 120 g of camellia oil was added, heated to 140 ° C and stirred, then cooled to room temperature, filtered, and the filtrate was defoamed with a defoaming agent emulsified silicone oil to obtain a modified viscose fiber primary stock solution.
[0049] c. In an ice-water mixture, add 25 g of flake graphite to 300 mL of concentrated sulfuric acid, slowly add 100 g of potassium permanganate while stirring, and store at a temperature below 5°C for 80 h. Then add it to 1000 mL of deionized water, stir and react at a temperature below 35°C for 3 h, heat to 100°C and react for 3 h, then add 50 mL of 30% hydrogen peroxide and let stand for 16 h. Wash with 5% hydrochloric acid and deionized water, and dry to obtain graphene oxide.
[0050] d. Add 50 g of 4-aminophenol to 700 mL of water, stir evenly, add 60 g of 2,3-epoxypropyltrimethylammonium chloride and 5 g of sodium hydroxide, heat to 150°C, and react with continuous stirring for 5 h to obtain 4-aminophenol grafted quaternary ammonium salt; add graphene oxide to 500 mL of dimethylformamide and stir evenly, ultrasonically treat for 1 h to obtain a graphene oxide suspension, then add 4-aminophenol grafted quaternary ammonium salt and 30 g of dicyclohexylcarbocyanine, ultrasonically treat for 5 min, react at 150°C for 50 h, add anhydrous ethanol and let stand overnight, remove the upper clear night, filter the lower precipitate with a polytetrafluoroethylene membrane, wash with ethanol and deionized water, and dry to obtain modified graphene oxide.
[0051] e. Add 50 g of modified viscose fiber primary stock solution into a high-pressure reactor, add 15 g of modified graphene oxide, seal it, react at 170°C for 18 h, take it out and wash it 5 times with 75°C distilled water, dry it to constant weight, and spin it into long and thin fibers on a spinning machine. After water cooling, pulling, spinning, acid coagulation, stretching, curing with a curing agent, washing, and drying processes, viscose fibers containing camellia seed oil are obtained.
[0052] Comparative Example 1: Ordinary viscose fiber.
[0053] Comparative Example 2: No camellia seed oil was added, and the preparation method was the same as that of Example 1.
[0054] Performance Testing:
[0055] The combustion performance was tested according to the method of GB / 5455-85. The results are shown in Table 1.
[0056] The antibacterial properties were tested on Staphylococcus aureus, Escherichia coli, and Candida albicans, and the size of the inhibition zone was measured. The results are shown in Table 2;
[0057] The tensile test was carried out, and the results are shown in Table 3;
[0058] The viscose fibers of Examples 1 to 5 and Comparative Examples 1 to 2 were made into adult diapers through a spinning process, and 70 volunteers were selected to conduct a wearing experience test, with a 0 to 10 point system. The results were averaged, and the results are shown in Table 4.
[0059] Table 1: GB / 5455-85 combustion performance test data
[0060]
[0061] Table 2: Antibacterial performance test
[0062]
[0063] Table 3: Tensile test
[0064]
[0065] Table 4 Wearing experience experimental results
[0066]
[0067] It can be seen from Tables 1, 2, 3 and 4 that the flame retardant, antibacterial, anti-inflammatory and tensile properties of Examples 1 to 5 are better than those of the comparative example. At the same time, the fiber body feel of Examples 1 to 5 is better, and the produced diapers are more easily accepted.
[0068] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
[0069] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing viscose fiber containing camellia seed oil, characterized in that: The preparation method is as follows: a. Under pressure, heat azelaic acid to a molten state, add p-phenylenediamine, stir and react for 2-6 hours, reduce the pressure to atmospheric pressure at 1 MPa / h to obtain molten polyamide; add 3,5-dibromophenol to the methanol solution, stir and dissolve, heat to 50-60°C, add molten polyamide thereto, add initiator ammonium persulfate, heat to 80-120°C, react for 3-8 hours, stop the reaction, and cool to room temperature to obtain modified polyamide; b. The modified polyamide is mixed with the viscose stock solution, camellia oil is added, heated to 100-150°C, stirred and mixed, then cooled to room temperature, filtered, and the filtrate is defoamed with a defoaming agent to obtain a modified viscose fiber primary stock solution; c. In an ice-water mixture, add flake graphite to concentrated sulfuric acid, slowly add potassium permanganate while stirring, store at a temperature below 5°C for 50-100 h, then add it to deionized water, stir and react at a temperature below 35°C for 1-5 h, heat to 90-100°C and react for 1-3 h, then add 30% hydrogen peroxide and let stand for 10-20 h, wash with 5% hydrochloric acid and deionized water, and dry to obtain graphene oxide; d. Add 4-aminophenol to water, stir evenly, add 2,3-epoxypropyltrimethylammonium chloride and sodium hydroxide, heat to 100-150°C, and stir continuously for 1-5 h to obtain 4-aminophenol grafted quaternary ammonium salt; add graphene oxide to dimethylformamide, stir evenly, and ultrasonically treat for 1-2 h to obtain a graphene oxide suspension, then add 4-aminophenol grafted quaternary ammonium salt and dicyclohexylcarbocyanide, ultrasonically treat for 5-10 min, react at 120-150°C for 30-60 h, add anhydrous ethanol and let stand overnight, remove the upper clear night, filter the lower precipitate with a polytetrafluoroethylene membrane, wash with ethanol and deionized water, and dry to obtain modified graphene oxide; e. Add the modified viscose fiber primary stock solution into a high-pressure reactor, add modified graphene oxide, seal it, react at 140-180°C for 10-20 h, take it out and wash it with 60-80°C distilled water for 3-6 times, dry it to constant weight, and spin it into long and thin fibers on a spinning machine. After water cooling, pulling, spinning, acid coagulation, stretching, curing with a curing agent, washing, and drying processes, viscose fibers containing camellia seed oil are obtained.
2. The method for preparing a viscose fiber containing camellia oil according to claim 1, characterized in that: In the step a, the mass ratio of azelaic acid, p-phenylenediamine, 3,5-dibromophenol and initiator ammonium persulfate is 1:0.8-1.2:0.3-0.6:0.01-0.
03.
3. The method for preparing a viscose fiber containing camellia oil according to claim 1, characterized in that: In the step b, the mass ratio of the modified polyamide, viscose stock solution and camellia oil is 1:10-30:1-15.
4. The method for preparing a viscose fiber containing camellia oil according to claim 1, characterized in that: The defoaming agent in step b is one of emulsified silicone oil, polyoxyethylene polyoxypropylene pentaerythritol ether, and polyoxyethylene polyoxypropanolamine ether.
5. The method for preparing a viscose fiber containing camellia oil according to claim 1, characterized in that: In the step c, the mass ratio of flake graphite, concentrated sulfuric acid, potassium permanganate and 30% hydrogen peroxide is 1:10-25:2-5:1.5-3.
6. The method for preparing a viscose fiber containing camellia oil according to claim 1, characterized in that: In the step d, the mass ratio of 4-aminophenol, 2,3-epoxypropyltrimethylammonium chloride, sodium hydroxide and dicyclohexylcarboximide is 1:0.6-1.2:0.05-0.1:0.2-0.
6.
7. The method for preparing a viscose fiber containing camellia oil according to claim 1, characterized in that: In the step e, the mass ratio of the modified viscose fiber primary solution to the modified graphene oxide is 1:0.05-0.
3.
8. The viscose fiber containing camellia seed oil obtained by the method for preparing viscose fiber containing camellia seed oil according to claim 1, characterized in that: Application of the camellia seed oil-containing viscose fiber in diaper materials.