A method and application of synergistically utilizing garbage incineration fly ash and garbage leachate to prepare highly efficient heavy metal adsorbing activated carbon

By hydrothermally treating phosphate, printing and dyeing sludge and garbage incineration fly ash with oxidants and landfill leachate, efficient heavy metal adsorbent activated carbon is generated, which solves the problem of treating waste incineration fly ash and landfill leachate and achieves efficient removal of mercury, The effects of heavy metal contaminants such as arsenic and thallium.

CN118403616BActive Publication Date: 2024-10-25CHANGSHU INSTITUTE OF TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410881956.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-10-25
Estimated Expiration
2044-07-03

AI Technical Summary

Technical Problem

Improper treatment of waste incineration fly ash and landfill leachate can lead to environmental pollution, and existing technology makes it difficult to effectively utilize the resource value of these materials.

Method used

By mixing phosphate, printing and dyeing sludge and garbage incineration fly ash, combined with oxidants and landfill leachate for hydrothermal treatment, efficient heavy metal adsorbent activated carbon is generated. The hydrothermal and carbonization process is used to form a porous structure and load organic functional groups to achieve the removal of heavy metals. Stable adsorption.

Benefits of technology

The prepared activated carbon has a high specific surface area and significant heavy metal adsorption capacity, and can effectively remove heavy metal pollutants such as mercury, arsenic, and thallium. The process is simple and makes full use of the components of waste incineration fly ash and landfill leachate.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118403616B_ABST
    Figure CN118403616B_ABST
Patent Text Reader

Abstract

The present invention discloses a method and application of preparing highly efficient heavy metal adsorbing activated carbon by synergistically utilizing fly ash from garbage incineration and leachate. The method of the present invention has a simple preparation process, can fully and synergistically utilize the components of fly ash from garbage incineration and leachate, and realizes the preparation of activated carbon adsorbent through hydrothermal preoxidation and carbonization process. The prepared activated carbon adsorbent has a maximum specific surface area of ​​1164m 2 / g, the maximum adsorption capacity of heavy metals mercury, arsenic and thallium are 304mg / g, 145mg / g and 78mg / g respectively.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of harmless disposal and resource utilization of hazardous wastes, and in particular to a method for preparing highly efficient heavy metal adsorbing activated carbon by synergistically utilizing waste incineration fly ash and waste leachate, and its application. Background Art

[0002] Secondary pollutants such as fly ash and leachate generated during the incineration of garbage will cause serious harm to the environment if not properly handled. The amount of fly ash produced accounts for about 2.5% to 3% of the total amount of garbage, and its composition is complex, including various metal oxides, non-metal oxides, silicates, carbonates, etc. Fly ash contains a high concentration of heavy metal pollutants, which will cause serious pollution to water bodies, soil and organisms once they enter the environment. Fly ash also contains a small amount of persistent organic pollutants such as dioxins and furans. These pollutants are extremely toxic and bioaccumulative, posing a serious threat to human health. Some fly ash from garbage incineration may contain radioactive substances, such as uranium and thorium, which pose a potential threat to the environment and human health.

[0003] Leachate refers to a high-concentration organic wastewater that comes from the water contained in the garbage itself in the landfill, the rain and snow water entering the landfill, and other water, minus the saturated water holding capacity of the garbage and the overburden layer, and passes through the garbage layer and the overburden layer. The amount of leachate produced is related to factors such as the type of garbage, moisture content, and landfill time. During the landfill process, the organic matter in the garbage decomposes under the action of microorganisms, producing a large amount of leachate. The leachate contains high concentrations of pollutants such as organic matter, heavy metals, and microorganisms. If it is discharged directly without treatment, it will cause serious pollution to the surrounding water bodies. The pollutants in the leachate will enter the soil with rainwater, etc., change the composition and structure of the soil, reduce soil fertility and moisture, and affect the growth and quality of crops. The leachate accumulates in the landfill for a long time, which will produce an unpleasant odor and have a serious impact on the living environment and air quality of surrounding residents.

[0004] In view of the environmental hazards of waste incineration fly ash and landfill leachate, it is of great significance to find an effective way to utilize them. Waste incineration fly ash contains a large amount of metal oxides and non-metal oxides, which have good adsorption properties; while landfill leachate contains a large amount of organic matter and inorganic salts, which can react chemically with the oxides in the fly ash to form new compounds or complexes. Therefore, from the perspective of material composition, it is feasible to use waste incineration fly ash and landfill leachate to prepare high-efficiency heavy metal adsorption materials. Summary of the invention

[0005] Purpose of the invention: The purpose of the present invention is to provide a method and application of synergistically utilizing waste incineration fly ash and landfill leachate to prepare highly efficient heavy metal adsorbing activated carbon.

[0006] Technical solution: The method of the present invention for preparing highly efficient heavy metal adsorbing activated carbon by synergistically utilizing waste incineration fly ash and waste leachate comprises the following steps:

[0007] (1) Phosphate, printing and dyeing sludge and waste incineration fly ash are mixed and stirred evenly to obtain phosphorus-doped fly ash;

[0008] (2) mixing the oxidant and the landfill leachate, stirring them evenly, and obtaining an oxidized pre-doped leachate;

[0009] (3) mixing the phosphorus-doped fly ash of step (2) and the oxidation pre-doped leachate of step (3), and heating them while stirring to obtain a loose slurry;

[0010] (4) drying and grinding the loose slurry to obtain loose powder; placing the loose powder in a carbonization furnace for carbonization to obtain carbonized slag;

[0011] (5) Mix water and carbonized slag, stir evenly, separate the solid and liquid, dry and grind the separated solid to obtain an activated carbon adsorbent.

[0012] Furthermore, the mass ratio of the phosphate, printing and dyeing sludge and waste incineration fly ash in step (1) is 0.5-5.5:15-55:100.

[0013] Furthermore, the phosphate described in step (1) is a mixture of any one or more of sodium hexametaphosphate, sodium pyrophosphate, sodium phosphate, disodium hydrogen phosphate, and sodium dihydrogen phosphate.

[0014] Furthermore, the mass ratio of the oxidant to the landfill leachate in step (2) is 0.5-4.5:100.

[0015] Furthermore, the oxidant in step (2) is a mixture of any one or more of sodium thiosulfate, ammonium persulfate, and potassium persulfate.

[0016] Furthermore, the mass ratio of the phosphorus-doped fly ash to the oxidation pre-doped leachate in step (3) is 20-60:100.

[0017] Furthermore, the heating method in step (3) is hydrothermal, the heating time is 0.5 to 2.5 hours, and the heating temperature is 80 to 240°C.

[0018] Furthermore, the drying temperature in step (4) is 50-150° C., the carbonization temperature is 350-750° C., and the carbonization time is 1.5-4.5 hours.

[0019] Furthermore, the liquid-to-solid ratio of water and carbonized slag in step (5) is 2-6:1 mL / g.

[0020] The activated carbon prepared by the above method of the present invention is used in purifying heavy metal pollutants.

[0021] Furthermore, the heavy metals include mercury, arsenic and thallium.

[0022] Reaction mechanism: During the hydrothermal process, under the catalytic action of inorganic salts contained in fly ash, printing and dyeing sludge, and landfill leachate, the added oxidant undergoes a violent redox reaction with some organic matter in the printing and dyeing sludge and landfill leachate to generate carbon dioxide, carbon dioxide free radicals, and carbonate. The released gas makes the slurry porous and fluffy, and the generated carbon dioxide free radicals can reduce some heavy metal ions. Carbonate can combine with calcium ions and heavy metal ions to form carbonate precipitation. At the same time, during the hydrothermal process, phosphate reacts with calcium-based materials, heavy metals in the fly ash of garbage incineration, and ammonia nitrogen in the landfill leachate to generate hydroxyapatite, chlorohydroxyapatite, and phosphate heavy metal precipitation micro-nano particles. The generated hydroxyapatite and chlorohydroxyapatite micro-nano particles can also adsorb heavy metal ions through ion exchange, thereby stabilizing heavy metal ions. The loose powder is placed in a carbonization furnace. Under high temperature, the pre-oxidized organic matter in the printing and dyeing sludge and landfill leachate undergoes a more complete carbonization reaction under the etching of inorganic salts, generating a loose porous carbon-based surface loaded with organic functional groups. At the same time, the hydroxyapatite and chlorohydroxyapatite formed in the hydrothermal process and the residual free ammonium and free phosphorus in the landfill leachate are adsorbed on the carbon surface to form more adsorption active sites. At the same time, during the carbonization process, the calcium-based materials in the fly ash further react with the dissolved chloride salts in the printing and dyeing sludge and landfill leachate to generate calcium chloride. The unbound heavy metals and a small amount of aluminum and iron in the fly ash and some inorganic cations in the printing and dyeing sludge and landfill leachate react with the chloride salts on the carbon-based surface to form chloride gas for removal. Mix water and carbonized slag, and the unreacted inorganic salts doped in the carbonized slag during the stirring process are dissolved in the water. After solid-liquid separation and drying, high-efficiency heavy metal adsorption activated carbon is obtained.

[0023] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: the method of the present invention has a simple preparation process, can fully and synergistically utilize the waste incineration fly ash and waste leachate components, and realizes the preparation of activated carbon adsorbent through hydrothermal preoxidation and carbonization process. The maximum specific surface area of ​​the prepared activated carbon adsorbent is 1164m 2 / g, the maximum adsorption capacity of heavy metals mercury, arsenic and thallium are 304mg / g, 145mg / g and 78mg / g respectively. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 It is a flow chart of the present invention. DETAILED DESCRIPTION

[0025] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.

[0026] Waste incineration fly ash: Waste incineration fly ash is provided by the Second Municipal Waste Incineration Power Plant in Changshu, Jiangsu Province, mainly including 38.14% CaO, 24.05% Cl, 10.21% SO3, 12.15% Na2O, 6.21% K2O, 3.17% SiO2, 1.41% Fe2O3, 1.19% Al2O3 and other components (loss on ignition and other inevitable impurities);

[0027] Printing and dyeing sludge: Printing and dyeing sludge is provided by Shaoxing Keqiao Tianyu Printing and Dyeing Co., Ltd. Its chemical composition mainly includes 43.86% SO3, 36.34% Fe2O3, 7.01% SiO2, 5.82% Al2O3, 2.93% CaO and other components (loss on ignition and other inevitable impurities);

[0028] Landfill leachate: The landfill leachate used in the experiment was obtained from Zhuji Sanfeng Environmental Protection Energy Co., Ltd. The COD mass concentration of this batch of concentrated landfill leachate was 3639 mg / L, the total phosphorus concentration was 294 mg / L, and the ammonia nitrogen concentration was 1062 mg / L.

[0029] Example 1 Effect of the mass ratio of phosphate, printing and dyeing sludge and waste incineration fly ash on the performance of the prepared activated carbon adsorbent

[0030] According to the mass ratio of 0.25:15:100, 0.3:15:100, 0.4:15:100, 0.5:7.5:100, 0.5:10:100, 0.5:12.5:100, 0.5:15:100, 3:15:100, 5.5:15:100, 0.5:35:100, 3:35:100, 5.5:35:10 0, 0.5:55:100, 3:55:100, 5.5:55:100, 5.5:60:100, 5.5:65:100, 5.5:70:100, 6:55:100, 6.5:55:100, 7:55:100 Phosphate, printing and dyeing sludge and waste incineration fly ash are mixed and stirred evenly to obtain phosphorus-doped fly ash, wherein the phosphate is sodium hexametaphosphate. Oxidant and landfill leachate are mixed in a mass ratio of 0.5:100 and stirred evenly to obtain oxidation pre-doped leachate, wherein the oxidant is sodium thiosulfate. Phosphorus-doped fly ash and oxidation pre-doped leachate are mixed in a mass ratio of 20:100, heated while stirring, and hydrothermally heated for 0.5 hours to obtain loose mortar, wherein the heating temperature is 80°C. The loose mortar is dried and ground to obtain loose powder, wherein the drying temperature is 50°C. The loose powder is placed in a carbonization furnace for carbonization to obtain carbonized slag, wherein the carbonization temperature is 350°C and the carbonization time is 1.5 hours. Water and carbonized slag are mixed according to a liquid-solid ratio of 2:1 mL / g, stirred evenly, and then solid-liquid separation is performed, and the separated solid is dried and ground to obtain an activated carbon adsorbent.

[0031] The activated carbon adsorbent prepared as above was used for the adsorption test of heavy metals mercury, arsenic and thallium. Specifically, 0.5g of activated carbon adsorbent was weighed and put into 1L of mercury, arsenic and thallium solution, stirred for 30 minutes, filtered, and the treated waste liquid was obtained. The initial mercury, arsenic and thallium concentrations of the mercury-containing solution were 250mg / L, 250mg / L and 100mg / L, respectively. The concentrations of dissolved mercury and arsenic in the solution were determined according to the standard "Determination of Mercury, Arsenic, Selenium, Bismuth and Antimony in Water Quality by Atomic Fluorescence Method" (HJ 695-2014); the concentration of thallium in the leaching solution was determined according to the standard "Determination of Thallium in Water Quality by Graphite Furnace Atomic Absorption Spectrophotometry" (HJ 748-2015). The adsorption performance of the activated carbon adsorbent was calculated according to formula (1), where, is the adsorption capacity of mercury, arsenic or thallium on activated carbon adsorbent, mg / g, and are the concentrations of dissolved mercury, arsenic or thallium in the solution before and after the adsorption experiment in mg / L, V is the volume of the solution containing mercury, arsenic or thallium in L (1L), and m is the dosage of activated carbon adsorbent (1g).

[0032] (1)

[0033] The specific surface area of ​​the activated carbon adsorbent prepared by the present invention is measured according to "Test Method for Specific Surface Area of ​​Coal-Based Granular Activated Carbon" (GB / T 7702.21-1997).

[0034] The results of the adsorption capacity test of the activated carbon adsorbent in this embodiment are shown in Table 1.

[0035] Table 1 Effect of mass ratio of phosphate, printing and dyeing sludge and waste incineration fly ash on the performance of prepared activated carbon adsorbent

[0036]

[0037] It can be seen from Table 1 that when the mass ratio of phosphate, printing and dyeing sludge and waste incineration fly ash is less than 0.5:15:100 (such as in Table 1, the mass ratio of phosphate, printing and dyeing sludge and waste incineration fly ash = 0.4:15:100, 0.3:15:100, 0.25:15:100, 0.5:12.5:100, 0.5:10:100, 0.5:7.5:100 and lower ratios not listed in Table 1), less phosphate and printing and dyeing sludge are added, and the phosphate, printing and dyeing sludge and waste incineration fly ash react insufficiently in the subsequent hydrothermal process, resulting in the specific surface area of ​​the prepared activated carbon adsorbent and the corresponding mercury, arsenic and thallium adsorption capacity are significantly reduced with the decrease of the mass ratio of phosphate, printing and dyeing sludge and waste incineration fly ash. When the mass ratio of phosphate, printing and dyeing sludge and waste incineration fly ash is equal to 0.5~5.5:15~55:100 (as in Table 1, the mass ratio of phosphate, printing and dyeing sludge and waste incineration fly ash = 0.5:15:100, 3:15:100, 5.5:15:100, 0.5:35:100, 3:35:100, 5.5:35:100, 0.5:55:100, 3:55:100, 5.5:55:100), during the hydrothermal process, under the catalytic action of inorganic salts contained in fly ash, printing and dyeing sludge and landfill leachate, the added oxidant undergoes a violent redox reaction with some organic matter in the printing and dyeing sludge and landfill leachate to generate carbon dioxide, carbon dioxide free radicals and carbonate. The released gas makes the slurry porous and fluffy, and the generated carbon dioxide free radicals can reduce some heavy metal ions. Carbonate can combine with calcium ions and heavy metal ions to form carbonate precipitation. At the same time, during the hydrothermal process, phosphate reacts with calcium-based materials, heavy metals in waste incineration fly ash and ammonia nitrogen in landfill leachate to generate hydroxyapatite, chlorohydroxyapatite and phosphate heavy metal precipitation micro-nanoparticles. The generated hydroxyapatite and chlorohydroxyapatite micro-nanoparticles can also adsorb heavy metal ions through ion exchange, thereby stabilizing heavy metal ions. Finally, the prepared activated carbon adsorbent has a specific surface area greater than 915.04m 2 / g, the mercury adsorption capacity is greater than 203mg / g, the arsenic adsorption capacity is greater than 106mg / g, and the thallium adsorption capacity is greater than 54mg / g. When the mass ratio of phosphate, printing and dyeing sludge and waste incineration fly ash is greater than 5.5:55:100 (such as in Table 1, the mass ratio of phosphate, printing and dyeing sludge and waste incineration fly ash = 5.5:60:100, 5.5:65:100, 5.5:70:100, 6:55:100, 6.5:55:100, 7:55:100 and higher ratios not listed in Table 1), phosphate and printing and dyeing sludge are added excessively, and the reaction between materials in the hydrothermal process is unbalanced, resulting in the specific surface area of ​​the prepared activated carbon adsorbent and the corresponding mercury, arsenic, and thallium adsorption capacities are significantly reduced as the mass ratio of phosphate, printing and dyeing sludge and waste incineration fly ash further increases.

[0038] Therefore, in summary, considering the benefits and costs, when the mass ratio of phosphate, printing and dyeing sludge and waste incineration fly ash is equal to 0.5~5.5:15~55:100, it is most conducive to improving the specific surface area and adsorption performance of the prepared heavy metal adsorbent.

[0039] Example 2 Effect of the mass ratio of oxidant to landfill leachate on the performance of the prepared activated carbon adsorbent

[0040] Phosphate, printing and dyeing sludge and waste incineration fly ash are mixed in a mass ratio of 5.5:55:100, stirred evenly, and phosphorus-doped fly ash is obtained, wherein the phosphate is sodium pyrophosphate. Oxidant and landfill leachate are mixed in a mass ratio of 0.25:100, 0.3:100, 0.4:100, 0.5:100, 2.5:100, 4.5:100, 5:100, 5.5:100, 6:100, stirred evenly, and oxidation pre-doped leachate is obtained, wherein the oxidant is ammonium persulfate. Phosphorus-doped fly ash and oxidation pre-doped leachate are mixed in a mass ratio of 40:100, heated while stirring, and hydrothermally heated for 1.5 hours to obtain loose mortar, wherein the heating temperature is 160°C. The loose mortar is dried and ground to obtain loose powder, wherein the drying temperature is 100°C. The loose powder is placed in a carbonization furnace for carbonization to obtain carbonized slag, wherein the carbonization temperature is 550°C and the carbonization time is 3 hours. Water and carbonized slag are mixed according to a liquid-solid ratio of 4:1 mL / g, stirred evenly, and then solid-liquid separation is performed, and the separated solid is dried and ground to obtain an activated carbon adsorbent.

[0041] The heavy metal mercury, arsenic, and thallium adsorption test, the calculation of the adsorption amount of mercury, arsenic, or thallium by the activated carbon adsorbent, and the determination of the specific surface area of ​​the activated carbon adsorbent are all the same as in Example 1.

[0042] The results of the adsorption capacity test of the activated carbon adsorbent in this example are shown in Table 2.

[0043] Table 2 Effect of the mass ratio of oxidant to landfill leachate on the performance of the prepared activated carbon adsorbent

[0044]

[0045] It can be seen from Table 2 that when the mass ratio of the oxidant to the leachate is less than 0.5:100 (such as in Table 2, the mass ratio of the oxidant to the leachate = 0.4:100, 0.3:100, 0.25:100 and lower ratios not listed in Table 2), less oxidant is added, and the oxidant and the leachate do not react fully in the subsequent hydrothermal process, resulting in the specific surface area of ​​the prepared activated carbon adsorbent and the corresponding mercury, arsenic and thallium adsorption capacities all significantly decreasing with the decrease in the mass ratio of the oxidant to the leachate. When the mass ratio of oxidant to landfill leachate is equal to 0.5~4.5:100 (as shown in Table 2, the mass ratio of oxidant to landfill leachate = 0.5:100, 2.5:100, 4.5:100), during the hydrothermal process, under the catalytic action of inorganic salts contained in fly ash, printing and dyeing sludge, and landfill leachate, the added oxidant undergoes a violent redox reaction with some organic matter in printing and dyeing sludge and landfill leachate to generate carbon dioxide, carbon dioxide free radicals, and carbonate. The released gas makes the slurry porous and fluffy, and the generated carbon dioxide free radicals can reduce some heavy metal ions. Carbonate can combine with calcium ions and heavy metal ions to form carbonate precipitation. At the same time, during the hydrothermal process, phosphate reacts with calcium-based materials, heavy metals in waste incineration fly ash, and ammonia nitrogen in landfill leachate to generate hydroxyapatite, chlorohydroxyapatite, and phosphate heavy metal precipitation micro-nano particles. The generated hydroxyapatite and chlorohydroxyapatite micro-nano particles can also adsorb heavy metal ions through ion exchange, thereby stabilizing heavy metal ions. Finally, the specific surface area of ​​the prepared activated carbon adsorbent is greater than 1004m 2 / g, the mercury adsorption capacity is greater than 241mg / g, the arsenic adsorption capacity is greater than 119mg / g, and the thallium adsorption capacity is greater than 66mg / g. When the mass ratio of oxidant to landfill leachate is greater than 4.5:100 (such as in Table 2, the mass ratio of oxidant to landfill leachate = 5:100, 5.5:100, 6:100 and higher ratios not listed in Table 2), the oxidant is added excessively, and the reaction between materials in the hydrothermal process is unbalanced, resulting in the specific surface area of ​​the prepared activated carbon adsorbent and the corresponding mercury, arsenic, and thallium adsorption capacities are significantly reduced as the mass ratio of oxidant to landfill leachate further increases.

[0046] Therefore, in summary, considering the benefits and costs, when the mass ratio of oxidant to leachate is equal to 0.5~4.5:100, it is most conducive to improving the specific surface area and adsorption performance of the prepared heavy metal adsorbent.

[0047] Example 3 Effect of the mass ratio of phosphorus-doped fly ash and oxidized pre-doped leachate on the performance of the prepared activated carbon adsorbent

[0048] Phosphate, printing and dyeing sludge and waste incineration fly ash are mixed in a mass ratio of 5.5:55:100, stirred evenly, and phosphorus-doped fly ash is obtained, wherein the phosphate is sodium phosphate. Oxidant and landfill leachate are mixed in a mass ratio of 4.5:100, stirred evenly, and oxidation pre-doped leachate is obtained, wherein the oxidant is potassium persulfate. Phosphorus-doped fly ash and oxidation pre-doped leachate are mixed in a mass ratio of 12.5:100, 15:100, 17.5:100, 20:100, 40:100, 60:100, 65:100, 70:100, 75:100, heated while stirring, hydrothermally heated for 2.5 hours, and loose mortar is obtained, wherein the heating temperature is 240°C. The loose mortar is dried and ground to obtain loose powder, wherein the drying temperature is 150°C. The loose powder is placed in a carbonization furnace for carbonization to obtain carbonized slag, wherein the carbonization temperature is 750°C and the carbonization time is 4.5 hours. Water and carbonized slag are mixed according to a liquid-solid ratio of 6:1 mL / g, stirred evenly, and then solid-liquid separation is performed, and the separated solid is dried and ground to obtain an activated carbon adsorbent.

[0049] The heavy metal mercury, arsenic, and thallium adsorption test, the calculation of the adsorption amount of mercury, arsenic, or thallium by the activated carbon adsorbent, and the determination of the specific surface area of ​​the activated carbon adsorbent are all the same as in Example 1.

[0050] The results of the adsorption capacity test of the activated carbon adsorbent in this example are shown in Table 3.

[0051] Table 3 Effect of the mass ratio of phosphorus-doped fly ash and oxidized pre-doped leachate on the performance of the prepared activated carbon adsorbent

[0052]

[0053] It can be seen from Table 3 that when the mass ratio of phosphorus-doped fly ash and oxidized pre-doped leachate is less than 20:100 (such as in Table 3, the mass ratio of phosphorus-doped fly ash and oxidized pre-doped leachate = 17.5:100, 15:100, 12.5:100 and lower ratios not listed in Table 3), the addition of phosphorus-doped fly ash is small, and the reaction of phosphorus-doped fly ash and oxidized pre-doped leachate in the subsequent hydrothermal process is insufficient, resulting in the specific surface area of ​​the prepared activated carbon adsorbent and the corresponding mercury, arsenic and thallium adsorption capacities all significantly decreasing with the decrease of the mass ratio of phosphorus-doped fly ash and oxidized pre-doped leachate. When the mass ratio of phosphorus-doped fly ash and oxidized pre-doped leachate is equal to 20~60:100 (as shown in Table 3, the mass ratio of phosphorus-doped fly ash and oxidized pre-doped leachate = 20:100, 40:100, 60:100), during the hydrothermal process, under the catalytic action of inorganic salts contained in fly ash, printing and dyeing sludge, and landfill leachate, the added oxidant undergoes a violent redox reaction with some organic matter in printing and dyeing sludge and landfill leachate to generate carbon dioxide, carbon dioxide free radicals, and carbonate. The released gas makes the slurry porous and fluffy, and the generated carbon dioxide free radicals can reduce some heavy metal ions. Carbonate can combine with calcium ions and heavy metal ions to form carbonate precipitation. At the same time, during the hydrothermal process, phosphate reacts with calcium-based materials, heavy metals in waste incineration fly ash, and ammonia nitrogen in landfill leachate to generate hydroxyapatite, chlorohydroxyapatite, and phosphate heavy metal precipitation micro-nano particles. The generated hydroxyapatite and chlorohydroxyapatite micro-nano particles can also adsorb heavy metal ions through ion exchange, thereby stabilizing heavy metal ions. Finally, the prepared activated carbon adsorbent has a specific surface area greater than 1102 m 2 / g, the mercury adsorption capacity is greater than 272mg / g, the arsenic adsorption capacity is greater than 132mg / g, and the thallium adsorption capacity is greater than 74mg / g. When the mass ratio of phosphorus-doped fly ash to oxidation pre-doped leachate is greater than 60:100 (such as in Table 3, the mass ratio of phosphorus-doped fly ash to oxidation pre-doped leachate = 65:100, 70:100, 75:100 and higher ratios not listed in Table 3), the oxidant is added excessively, and the reaction between materials in the hydrothermal process is unbalanced, resulting in the specific surface area of ​​the prepared activated carbon adsorbent and the corresponding mercury, arsenic, and thallium adsorption capacities are significantly reduced as the mass ratio of phosphorus-doped fly ash to oxidation pre-doped leachate further increases.

[0054] Therefore, in summary, considering the benefits and costs, when the mass ratio of phosphorus-doped fly ash and oxidation pre-doped leachate is equal to 20~60:100, it is most conducive to improving the specific surface area and adsorption performance of the prepared heavy metal adsorbent.

[0055] Example 4 Effect of Phosphate Type on the Performance of Prepared Activated Carbon Adsorbent

[0056] Phosphate, printing and dyeing sludge and waste incineration fly ash are mixed in a mass ratio of 5.5:55:100, stirred evenly, and phosphorus-doped fly ash is obtained, wherein the phosphate is any one of sodium hexametaphosphate, sodium pyrophosphate, sodium phosphate, disodium hydrogen phosphate, and sodium dihydrogen phosphate. Oxidant and landfill leachate are mixed in a mass ratio of 4.5:100, stirred evenly, and oxidation pre-doped leachate is obtained, wherein the oxidant is potassium persulfate. Phosphorus-doped fly ash and oxidation pre-doped leachate are mixed in a mass ratio of 60:100, heated while stirring, and hydrothermally heated for 2.5 hours to obtain loose mortar, wherein the heating temperature is 240°C. The loose mortar is dried and ground to obtain loose powder, wherein the drying temperature is 150°C. The loose powder is placed in a carbonization furnace for carbonization to obtain carbonized slag, wherein the carbonization temperature is 750°C and the carbonization time is 4.5 hours. Water and carbonized slag are mixed at a liquid-solid ratio of 6:1 mL / g, stirred evenly, and then solid-liquid separation is performed. The separated solid is dried and ground to obtain an activated carbon adsorbent.

[0057] The heavy metal mercury, arsenic, and thallium adsorption test, the calculation of the adsorption amount of mercury, arsenic, or thallium by the activated carbon adsorbent, and the determination of the specific surface area of ​​the activated carbon adsorbent are all the same as in Example 1.

[0058] The results of the adsorption capacity test of the activated carbon adsorbent in this example are shown in Table 4.

[0059] Table 4 Effect of phosphate type on the performance of prepared activated carbon adsorbent

[0060]

[0061] It can be seen from Table 4 that when the phosphate is any one of sodium hexametaphosphate, sodium pyrophosphate, sodium phosphate, disodium hydrogen phosphate, and sodium dihydrogen phosphate, there is no significant difference in the specific surface area and adsorption performance of the prepared heavy metal adsorbent.

[0062] Comparative example of the effects of different processes on the performance of the prepared activated carbon adsorbent

[0063] The process of the present invention is as follows: phosphate, printing and dyeing sludge and waste incineration fly ash are mixed in a mass ratio of 5.5:55:100, stirred evenly, and phosphorus-doped fly ash is obtained, wherein the phosphate is sodium dihydrogen phosphate. The oxidant and the landfill leachate are mixed in a mass ratio of 4.5:100, stirred evenly, and an oxidation pre-doped leachate is obtained, wherein the oxidant is potassium persulfate. The phosphorus-doped fly ash and the oxidation pre-doped leachate are mixed in a mass ratio of 60:100, heated while stirring, and hydrothermally heated for 2.5 hours to obtain a loose mortar, wherein the heating temperature is 240°C. The loose mortar is dried and ground to obtain a loose powder, wherein the drying temperature is 150°C. The loose powder is placed in a carbonization furnace for carbonization to obtain carbonized slag, wherein the carbonization temperature is 750°C and the carbonization time is 4.5 hours. Water and carbonized slag are mixed in a liquid-solid ratio of 6:1 mL / g, stirred evenly, and then solid-liquid separation is performed, and the separated solid is dried and ground to obtain an activated carbon adsorbent.

[0064] Comparative process 1: Phosphate, printing and dyeing sludge and waste incineration fly ash are mixed in a mass ratio of 5.5:55:100, stirred evenly, and phosphorus-doped fly ash is obtained, wherein the phosphate is sodium dihydrogen phosphate. Phosphorus-doped fly ash and landfill leachate are mixed in a mass ratio of 60:100, heated while stirring, and hydrothermally heated for 2.5 hours to obtain loose slurry, wherein the heating temperature is 240°C. The loose slurry is dried and ground to obtain loose powder, wherein the drying temperature is 150°C. The loose powder is placed in a carbonization furnace for carbonization to obtain carbonized slag, wherein the carbonization temperature is 750°C and the carbonization time is 4.5 hours. Water and carbonized slag are mixed in a liquid-solid ratio of 6:1mL / g, stirred evenly, and then solid-liquid separation is performed, and the separated solid is dried and ground to obtain an activated carbon adsorbent.

[0065] Comparative process 2: Mix the oxidant and the landfill leachate in a mass ratio of 4.5:100, stir evenly, and obtain an oxidized pre-doped leachate, wherein the oxidant is potassium persulfate. Mix the waste incineration fly ash and the oxidized pre-doped leachate in a mass ratio of 60:100, heat while stirring, and hydrothermally heat for 2.5 hours to obtain a loose slurry, wherein the heating temperature is 240°C. Dry the loose slurry, grind it into powder, and obtain a loose powder, wherein the drying temperature is 150°C. Place the loose powder in a carbonization furnace for carbonization to obtain carbonized slag, wherein the carbonization temperature is 750°C and the carbonization time is 4.5 hours. Mix water and carbonized slag in a liquid-solid ratio of 6:1mL / g, stir evenly, and then perform solid-liquid separation, dry the separated solid, grind it into powder, and obtain an activated carbon adsorbent.

[0066] The heavy metal mercury, arsenic, and thallium adsorption test, the calculation of the adsorption amount of mercury, arsenic, or thallium by the activated carbon adsorbent, and the determination of the specific surface area of ​​the activated carbon adsorbent are all the same as in Example 1.

[0067] The results of the adsorption capacity test of the activated carbon adsorbent in this comparative example are shown in Table 5.

[0068] Table 5 Effects of different processes on the performance of the prepared activated carbon adsorbent

[0069]

[0070] It can be seen from Table 5 that the specific surface area and adsorption performance of the activated carbon prepared by the process of the present invention are significantly better than those of comparative process 1 and comparative process 2.

Claims

1. A method for preparing highly efficient heavy metal adsorbing activated carbon by synergistically utilizing waste incineration fly ash and landfill leachate, characterized in that: The following steps are involved: (1) Phosphate, printing and dyeing sludge and waste incineration fly ash are mixed and stirred evenly to obtain phosphorus-doped fly ash; The mass ratio of the phosphate, printing and dyeing sludge and waste incineration fly ash is 0.5-5.5:15-55:100; (2) mixing the oxidant and the landfill leachate, stirring them evenly, and obtaining an oxidized pre-doped leachate; The mass ratio of the oxidant to the landfill leachate is 0.5-4.5:100; (3) mixing the phosphorus-doped fly ash of step (2) and the oxidation pre-doped leachate of step (3), and heating them while stirring to obtain a loose slurry; The mass ratio of the phosphorus-doped fly ash to the oxidized pre-doped leachate is 20-60:100; (4) drying and grinding the loose slurry to obtain loose powder; placing the loose powder in a carbonization furnace for carbonization to obtain carbonized slag; (5) Mix water and carbonized slag, stir evenly, separate the solid and liquid, dry and grind the separated solid to obtain an activated carbon adsorbent.

2. The method according to claim 1, characterized in that The phosphate described in step (1) is any one or more of sodium hexametaphosphate, sodium pyrophosphate, sodium phosphate, disodium hydrogen phosphate, and sodium dihydrogen phosphate.

3. The method according to claim 1, characterized in that: The oxidant in step (2) is a mixture of any one or more of sodium thiosulfate, ammonium persulfate and potassium persulfate.

4. The method according to claim 1, characterized in that: In step (3), the heating method is hydrothermal, the heating time is 0.5 to 2.5 hours, and the heating temperature is 80 to 240°C.

5. The method according to claim 1, characterized in that The drying temperature in step (4) is 50-150° C., the carbonization temperature is 350-750° C., and the carbonization time is 1.5-4.5 hours.

6. The method according to claim 1, characterized in that The liquid-to-solid ratio of water to carbonized slag in step (5) is 2-6:1 mL / g.

7. Use of the activated carbon prepared by the method according to any one of claims 1 to 6 in purifying heavy metal pollutants.

8. The use according to claim 7, characterized in that: The heavy metals include mercury, arsenic and thallium.