A high-strength exterior wall insulation board and preparation method thereof
By using modified xonotlite powder and perovskite powder in exterior wall insulation boards, a porous surface and low surface energy agglomerated microsphere structure are formed, which solves the problem of existing technology being difficult to meet diversified needs and achieves high strength, low heat conductivity, excellent waterproofing, moisture absorption resistance and weather resistance, meeting the composite performance requirements of the construction market.
Patent Information
- Application Number
- CN202410653362.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-24
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-05-24
AI Technical Summary
When faced with diversified composite demands, existing exterior wall insulation panels are unable to simultaneously meet performance requirements such as strength, waterproofing, weather resistance, chemical corrosion resistance and ultraviolet light resistance, and cannot effectively meet the diverse needs of the construction market.
Modified xonotlite powder and modified perovskite powder are used as fillers. Through modification treatment, a rough porous surface and a low surface energy agglomerated microsphere structure are formed to improve the mechanical, thermal insulation, waterproof and weather resistance properties of the insulation board, and through Zinc frame structure enhances UV light absorption and waterproof performance.
It significantly improves the thermal insulation performance, weather resistance, mechanical properties and waterproof performance of the exterior wall insulation board, extends its service life, avoids oxidative yellowing and deterioration loss, and meets the requirements of the construction market for diversified needs.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The present application relates to the field of thermal insulation boards, and in particular to a high-strength exterior wall thermal insulation board and a preparation method thereof. Background Art
[0002] Building energy conservation is an important part of my country's energy conservation work. There are many types of external insulation materials used for building exterior walls, including inorganic materials, organic materials, composite materials, etc.; the insulation materials used for beams, columns, shear walls and non-self-insulating masonry walls are all board or mortar insulation materials. The building exterior wall insulation system is a non-load-bearing insulation structure assembly composed of insulation boards, protective layers, and fixing materials and suitable for installation on the outer surface of the exterior wall. Currently, commonly used insulation boards include inorganic insulation boards, organic insulation boards, and composite insulation boards.
[0003] With the improvement of people's living standards and the diversification of construction project requirements, higher requirements are also put forward for insulation boards used in building exterior walls and their preparation materials. In addition to the requirements for fireproof and heat-insulating performance of insulation boards, further requirements such as waterproof, weather-resistant, chemical corrosion-resistant, UV-resistant and self-cleaning are put forward. However, although the existing exterior wall insulation boards are strong enough, they cannot effectively meet the diverse composite requirements. Therefore, the development of an exterior wall insulation board product that can meet the diverse composite requirements is crucial for the future construction market.
[0004] In order to solve the above-mentioned problems, the applicant provides a high-strength exterior wall insulation board and a preparation method thereof. The exterior wall insulation board prepared in the present application not only has excellent mechanical properties and low thermal conductivity, but also can further ensure its excellent waterproof, moisture absorption, weather resistance and light resistance, thereby meeting the existing diversified exterior wall insulation board needs and having very excellent market prospects. Summary of the invention
[0005] In order to solve the above problems, the first aspect of the present application provides a high-strength exterior wall insulation board, which comprises, by weight, 45 to 60 parts of cement slurry, 40 to 80 parts of lightweight aggregate, and 10 to 35 parts of additives.
[0006] As a preferred solution, the mass ratio of the cement slurry, lightweight aggregate and additive is (50-60): (55-70): (15-25).
[0007] As a preferred solution, the mass ratio of the cement slurry, lightweight aggregate and additive is (50-55): (60-65): (20-25).
[0008] As a preferred solution, the cement slurry comprises, by mass percentage, 40-45% cement, 10-20% fly ash, 10-20% filler powder, and the balance made up of gypsum.
[0009] As a preferred solution, the cement is at least one of ordinary Portland cement, sulphoaluminate cement and composite Portland cement.
[0010] As a preferred solution, the cement is ordinary Portland cement.
[0011] As a preferred solution, the cement is PO42.5.
[0012] As a preferred solution, the fly ash is sodium-containing fly ash.
[0013] As a preferred solution, the Na content of the sodium-containing fly ash is 1-3%.
[0014] As a preferred solution, the filling micropowder is modified xonotlite powder and modified perovskite powder.
[0015] As a preferred solution, the mass ratio of the modified xonotlite powder to the modified perovskite powder is (3-5): (1-1.5).
[0016] As a preferred solution, the mass ratio of the modified xonotlite powder to the modified perovskite powder is 4:1.
[0017] As a preferred scheme, the preparation method of the modified hard asphalt stone powder comprises the following steps: S1: adding hard asphalt stone powder to a reaction container, adding deionized water for stirring and dispersing; S2: heating to 80-90°C, adding phosphoric acid aqueous solution, stirring evenly and keeping warm for 2-3 hours to obtain a suspension of pretreated hard asphalt stone powder; S3: sequentially adding metal salt, alkali agent and silane coupling agent to the reaction container and mixing, cooling to 60-70°C for reaction for 3-4 hours, and maintaining the pH of the reaction system at 8-10; S4: after the reaction is completed, adding ethyl orthosilicate to the reaction container and continuously stirring, cooling to 50-55°C, reacting with 400-600W ultrasonic vibration for 1-2 hours, filtering, washing and drying after the reaction process to obtain modified hard asphalt stone powder.
[0018] As a preferred solution, the concentration of the phosphoric acid aqueous solution is 10-20wt%.
[0019] As a preferred solution, the mass ratio of the xonotlite powder and the phosphoric acid aqueous solution is (1-1.5):(2-3).
[0020] As a preferred solution, the mass ratio of the xonotlite powder, the metal salt and the silane coupling agent is (1-1.5): (0.5-1): (0.1-0.2).
[0021] As a preferred solution, the metal salts are magnesium chloride and aluminum chloride, and the mass ratio of the metal salts is (1-2): (1-2).
[0022] As a preferred solution, the amount of tetraethyl orthosilicate added is 5-10% of the mass of the S3 reaction solution system.
[0023] In the present application, the addition of modified xonotlite powder can greatly improve the thermal insulation performance of the exterior wall insulation board, and further improve its weather resistance, mechanical and chemical corrosion resistance. The hydroxy calcium phosphate generated by the modified hard ascites stone powder can form a rough and stable shell layer on its surface together with the subsequently added tetraethyl orthosilicate and metal salts, and then a cross-linked structural layer of metal oxide is formed on the surface. The existence of this structural layer can not only greatly increase the contact thermal resistance of the hard ascites stone powder, but also form multiple surface pores and rough surface to reduce the effect of gas convection heat transfer; on the other hand, the multi-hydroxy rough porous surface in the structure of the modified hard ascites stone powder can form a thin hydration layer on the surface during use. The existence of this hydration layer makes it more difficult for external active molecules or corrosive substances to contact the insulation board, thereby isolating them outside the surface hydration layer and greatly improving the weather resistance and corrosion resistance; finally, the multi-hydroxy groups on the surface of the modified hard ascites stone powder can form a good hydrogen bond connection with the modified perovskite powder internally, thereby forming an internal connection site with good performance when external force acts, thereby effectively improving the mechanical properties.
[0024] As a preferred scheme, the preparation method of the modified perovskite powder comprises the following steps: S1: adding the perovskite powder to a DMF solution prepared with glutaric anhydride and a silane coupling agent, heating to 60-70°C, heating and stirring for 3-5 hours, and filtering and washing after completion to obtain the pretreated perovskite powder; S2: dissolving zinc acetate and 2-methylimidazole in methanol solvent to prepare a solution, mixing the zinc acetate solution with the pretreated perovskite powder, heating to 80-85°C after mixing evenly, and dripping 2-methylimidazole solution under stirring at a speed of 60-120 r / min for 1-1.5 hours. After the dripping is completed, triethylamine is added, and then the temperature is reduced to 60-75°C and kept warm for reaction for 3-4 hours; S3: after the reaction is completed, centrifugation is performed to collect the solid product, and then the solid product is washed with methanol for multiple times and dried to obtain the product.
[0025] As a preferred solution, the average particle size of the perovskite powder is 400-600 nm.
[0026] As a preferred solution, the mass ratio of the perovskite powder, glutaric anhydride and silane coupling agent is (1~2):(1~2):(0.3~0.5).
[0027] As a preferred solution, the mass ratio of the pretreated perovskite powder, zinc acetate, 2-methylimidazole and triethylamine is (1.5~2): (0.1~0.5): (0.5~1.5): (0.01~0.05).
[0028] As a preferred solution, the average particle size of the modified perovskite powder is 500-800 nm.
[0029] As a preferred solution, the gypsum is desulfurized gypsum or high-strength gypsum.
[0030] In this application, the added modified perovskite powder can greatly improve the UV resistance and waterproof and moisture absorption resistance of the exterior wall insulation board. The added perovskite powder can be bonded with the formed zinc framework structure through coordination bonding. After the composite structure is generated, the band gap distance of the perovskite and zinc framework structure will be effectively reduced, and the formed electron flow path can guide the carriers and electron holes to gather on the perovskite and zinc framework structure respectively under the illumination of the exterior wall insulation board, thereby maintaining a very high surface light energy receiving capacity during the long-term use of the insulation board, consuming more energy during the long-term ultraviolet illumination process, thereby avoiding the phenomenon of oxidation yellowing and deterioration loss of the insulation board; on the other hand, the low surface energy agglomerated microsphere structure formed by it can greatly increase the free resistance and free path of the external infiltrated water molecules inside the insulation board in the insulation board system, thereby avoiding the excessive water penetration caused by the formation of the surface hydration layer, and thus greatly enhancing the waterproof and moisture absorption resistance of the insulation board.
[0031] As a preferred solution, the lightweight aggregate comprises, by weight percentage, 80-90% hollow vitrified microspheres and 10-20% rice husk powder.
[0032] As a preferred solution, the mass ratio of the vitrified microbeads to the rice husk powder is 85:15.
[0033] As a preferred solution, the average particle size of the hollow vitrified microspheres is 100-250 μm.
[0034] As a preferred solution, the average particle size of the hollow vitrified microspheres is 120-180 μm.
[0035] As a preferred solution, the additives are calculated by mass percentage, and the raw materials include: 25-35% high molecular polymer, 0.5-1.5% stearic acid, 10-15% plasticizer, 0.1-1% antioxidant, 2-6% auxiliary agent, and the balance is made up of rubber material.
[0036] As a preferred solution, the high molecular polymer is ethylene-vinyl acetate copolymer.
[0037] As a preferred solution, the plasticizer is at least one of paraffin oil, glycerol, zinc stearate, and phthalates.
[0038] As a preferred solution, the plasticizer is dioctyl phthalate.
[0039] As a preferred solution, the antioxidant is at least one of antioxidant 2246, antioxidant MBT, antioxidant 4020, and antioxidant 1098.
[0040] As a preferred solution, the antioxidant is antioxidant 2246.
[0041] As a preferred solution, the auxiliary agent is dinitrosopentamethylenetetramine and zinc dibutyldithiocarbamate, and the mass ratio of the two is 2:1.
[0042] As a preferred solution, the rubber material is at least one of chloroprene rubber, EPDM rubber and butyl rubber.
[0043] As a preferred solution, the rubber material is chloroprene rubber.
[0044] The second aspect of the present application provides a method for preparing the above-mentioned high-strength exterior wall insulation board, and the preparation method comprises the following steps: S1: mixing cement slurry, lightweight aggregate and additives to obtain a mixture; S2: adding the mixture to a slurry mixer and mixing with appropriate water for 0.5 to 1 hour, injecting the mixture into an insulation board mold, heating and calendering it into shape, and curing it for 3 to 5 hours and drying it until the moisture content is ≤1wt%.
[0045] The beneficial effects of this application are:
[0046] 1. A high-strength exterior wall insulation board provided in the present application not only has excellent mechanical properties and low thermal conductivity, but also can further ensure its excellent waterproof, moisture absorption, weather resistance, light resistance and other properties, thereby meeting the needs of the existing diversified exterior wall insulation boards and having very excellent market prospects.
[0047] 2. A high-strength exterior wall insulation board provided in the present application can greatly improve the insulation performance of the exterior wall insulation board by adding modified hard calcium silicate powder, and further improve its weather resistance, mechanical and chemical corrosion resistance; the modified hard calcium silicate powder, the hydroxy calcium phosphate generated by it can form a rough and stable shell layer on its surface together with the subsequently added tetraethyl orthosilicate and metal salts and other substances, and then form a cross-linked structural layer of metal oxide on the surface. The presence of this structural layer can not only greatly increase the contact thermal resistance of the hard calcium silicate powder, but also form multiple surface pores and rough surfaces to reduce the effect of gas convection heat transfer; on the other hand, the multi-hydroxy rough porous surface present in the modified hard calcium silicate powder structure can form a thin hydration layer on the surface during use. The presence of this hydration layer makes it more difficult for external active molecules or corrosive substances to contact the insulation board.
[0048] 3. A high-strength exterior wall insulation board provided in the present application, wherein the modified perovskite powder added thereto can greatly improve the UV resistance, waterproof and moisture absorption resistance of the exterior wall insulation board; the added perovskite powder can be bonded with the formed zinc framework structure through coordination bonding, and after the composite structure is generated, the bandgap distance between the perovskite and the zinc framework structure will be effectively reduced, and the formed electron flow path can guide the carriers and electron holes to gather on the perovskite and zinc framework structure respectively under the illumination of the exterior wall insulation board, thereby maintaining an extremely high surface light energy receiving capacity during the long-term use of the insulation board, consuming more energy during long-term ultraviolet illumination, thereby avoiding the phenomenon of oxidation, yellowing, deterioration and loss of the insulation board; on the other hand, the low surface energy agglomerated microsphere structure formed therein can act inside the insulation board system to greatly increase the free resistance and free path of external infiltrating water molecules inside the insulation board.
[0049] 4. The high-strength exterior wall insulation board provided in this application has simple and easy-to-obtain raw materials, and the preparation method is easy to operate. There is no chemical reaction that obviously corrodes the preparation equipment. Therefore, in the subsequent large-scale production, the raw material cost and equipment maintenance cost can be effectively controlled, and it has a very excellent market application prospect. DETAILED DESCRIPTION
[0050] The following will further explain and demonstrate the technical solutions in the above invention content of this application in the form of specific implementation schemes. The following embodiments are only practical examples used to illustrate and explain the contents of the technical solutions in the specification, and should not limit the scope of the claims to be protected by this application. All technical products based on the technical solutions described in the invention content of this application should be included in the scope to be protected by this application.
[0051] In the following examples, unless otherwise specified, the raw materials are all commercially available products, or can be prepared by methods well known to those skilled in the art.
[0052] Example 1: Example 1 provides a high-strength exterior wall insulation board in the first aspect, wherein the raw materials include, by weight: 52 parts of cement slurry, 64 parts of lightweight aggregate, and 24 parts of additives.
[0053] The raw materials of cement slurry include, by mass percentage, 42% cement, 18% fly ash, 18% filler powder and the balance made up by gypsum.
[0054] The cement is ordinary Portland cement PO42.5.
[0055] The fly ash is sodium-containing fly ash, and the Na content of the sodium-containing fly ash is 2%.
[0056] The filling micro powder is modified xonotlite powder and modified perovskite powder; the mass ratio of the modified xonotlite powder to the modified perovskite powder is 4:1.
[0057] The preparation method of modified hard ascites stone powder comprises the following steps, measured by mass: S1: taking 12 parts of hard ascites stone powder and adding them into a reaction container, adding 150 parts of deionized water for stirring and dispersing; S2: heating to 85°C, adding 22 parts of 15wt% phosphoric acid aqueous solution, stirring evenly and keeping warm for 2h to obtain a suspension of pretreated hard ascites stone powder; S3: sequentially adding 6 parts of metal salt, 3 parts of sodium hydroxide and 2 parts of 3-aminopropyltriethoxysilane into the reaction container and mixing, cooling to 65°C and reacting for 3.5h, keeping the pH of the reaction system at 10; S4: after the reaction is completed, adding ethyl orthosilicate into the reaction container and stirring continuously, cooling to 55°C, reacting with 500W ultrasonic vibration for 2h, filtering, washing and drying after the reaction process to obtain modified hard ascites stone powder.
[0058] The metal salts are magnesium chloride and aluminum chloride, and the mass ratio of the two is 1.5:1.
[0059] The amount of ethyl orthosilicate added is 8% of the mass of the S3 reaction solution system.
[0060] The preparation method of modified perovskite powder includes the following steps, calculated by mass: S1: adding 1.5 parts of perovskite powder to 50 parts of DMF solution prepared with 1 part of glutaric anhydride and 0.4 parts of 3-aminopropyltriethoxysilane, heating to 60°C, heating and stirring for 3.5 hours, filtering and washing after completion to obtain pretreated perovskite powder; S2: dissolving 0.4 parts of zinc acetate and 1.2 parts of 2-methylimidazole in 20 parts of methanol solvent respectively to prepare a solution, mixing the zinc acetate solution with 1.5 parts of pretreated perovskite powder, heating to 80°C after mixing evenly, and dripping 2-methylimidazole solution under stirring at a speed of 800r / min, the dripping time is 1.5h, adding 0.03 parts of triethylamine after the dripping is completed, and then reducing the temperature to 65°C and keeping the temperature for reaction for 3h; S3: after the reaction is completed, centrifugation and filtration are performed to collect the solid product, and then the solid product is washed with methanol for multiple times and dried to obtain the product.
[0061] The average particle size of the perovskite powder is 500 nm.
[0062] The average particle size of the modified perovskite powder is 650 nm.
[0063] The gypsum is desulfurized gypsum, which was purchased from the desulfurized gypsum products sold by Hebei Chidi Mineral Products Co., Ltd.
[0064] The lightweight aggregate is calculated by mass percentage, and the raw materials include: 85% hollow vitrified microspheres and 15% rice husk powder.
[0065] Hollow vitrified microspheres were purchased from hollow vitrified microspheres sold by Shandong Lanting Environmental Protection Technology Co., Ltd., with an average particle size of 150 μm; rice husk powder was purchased from 500-mesh rice husk powder sold by Shijiazhuang Longyun Agricultural Technology Co., Ltd.
[0066] The additives are calculated by weight percentage, and the raw materials include: 30% high molecular polymer, 1% stearic acid, 12% plasticizer, 0.5% antioxidant, 4% auxiliary agent, and the balance made up of rubber material.
[0067] The high molecular polymer is ethylene-vinyl acetate copolymer purchased from Guangzhou Hongcheng Plastic Chemical Co., Ltd. and sold as EVA1540 product.
[0068] The plasticizer is dioctyl phthalate.
[0069] The antioxidant is antioxidant 2246.
[0070] The auxiliary agents are dinitrosopentamethylenetetramine and zinc dibutyldithiocarbamate, and the mass ratio of the two is 2:1.
[0071] The rubber material is chloroprene rubber, which is purchased from Nippon Denka A-30 chloroprene rubber products.
[0072] The second aspect of the present embodiment provides a method for preparing the above-mentioned high-strength exterior wall insulation board, and the preparation method comprises the following steps: S1: mixing cement slurry, lightweight aggregate and additives to obtain a mixture; S2: adding the mixture to a slurry mixer and mixing with appropriate water for 1 hour, injecting the mixture into an insulation board mold, heating and calendering, and curing for 4 hours and drying the mixture until the moisture content is ≤1wt%.
[0073] Example 2: Example 2 provides a high-strength exterior wall insulation board in the first aspect, wherein the raw materials include, by weight: 55 parts of cement slurry, 55 parts of lightweight aggregate, and 20 parts of additives.
[0074] The raw materials of cement slurry include, by mass percentage, 45% cement, 12% fly ash, 20% filler powder and the balance made up by gypsum.
[0075] The cement is ordinary Portland cement PO42.5.
[0076] The fly ash is sodium-containing fly ash, and the Na content of the sodium-containing fly ash is 2%.
[0077] The filling micro powder is modified xonotlite powder and modified perovskite powder; the mass ratio of the modified xonotlite powder to the modified perovskite powder is 4.5:1.
[0078] The preparation method of modified hard ascites stone powder comprises the following steps, measured by mass: S1: taking 12 parts of hard ascites stone powder and adding them into a reaction container, adding 150 parts of deionized water for stirring and dispersing; S2: heating to 85°C, adding 22 parts of 15wt% phosphoric acid aqueous solution, stirring evenly and keeping warm for 2h to obtain a suspension of pretreated hard ascites stone powder; S3: sequentially adding 6 parts of metal salt, 3 parts of sodium hydroxide and 2 parts of 3-aminopropyltriethoxysilane into the reaction container and mixing, cooling to 65°C and reacting for 3.5h, keeping the pH of the reaction system at 10; S4: after the reaction is completed, adding ethyl orthosilicate into the reaction container and stirring continuously, cooling to 55°C, reacting with 500W ultrasonic vibration for 2h, filtering, washing and drying after the reaction process to obtain modified hard ascites stone powder.
[0079] The metal salts are magnesium chloride and aluminum chloride, and the mass ratio of the two is 1:1.
[0080] The amount of ethyl orthosilicate added is 10% of the mass of the S3 reaction solution system.
[0081] The preparation method of modified perovskite powder includes the following steps, calculated by mass: S1: adding 1.5 parts of perovskite powder to 50 parts of DMF solution prepared with 1 part of glutaric anhydride and 0.4 parts of 3-aminopropyltriethoxysilane, heating to 60°C, heating and stirring for 3.5 hours, filtering and washing after completion to obtain pretreated perovskite powder; S2: dissolving 0.4 parts of zinc acetate and 1.2 parts of 2-methylimidazole in 20 parts of methanol solvent respectively to prepare a solution, mixing the zinc acetate solution with 1.5 parts of pretreated perovskite powder, heating to 80°C after mixing evenly, and dripping 2-methylimidazole solution under stirring at a speed of 800r / min, the dripping time is 1.5h, adding 0.03 parts of triethylamine after the dripping is completed, and then reducing the temperature to 65°C and keeping the temperature for reaction for 3.5h; S3: after the reaction is completed, centrifugation and filtration are performed to collect the solid product, and then the solid product is washed with methanol for multiple times and dried to obtain the product.
[0082] The average particle size of the perovskite powder is 550 nm.
[0083] The average particle size of the modified perovskite powder is 720 nm.
[0084] The gypsum is desulfurized gypsum, which was purchased from the desulfurized gypsum products sold by Hebei Chidi Mineral Products Co., Ltd.
[0085] The lightweight aggregate is calculated by mass percentage, and the raw materials include: 85% hollow vitrified microspheres and 15% rice husk powder.
[0086] Hollow vitrified microspheres were purchased from hollow vitrified microspheres sold by Shandong Lanting Environmental Protection Technology Co., Ltd., with an average particle size of 150 μm; rice husk powder was purchased from 500-mesh rice husk powder sold by Shijiazhuang Longyun Agricultural Technology Co., Ltd.
[0087] The additives are calculated by weight percentage, and the raw materials include: 30% high molecular polymer, 1% stearic acid, 12% plasticizer, 0.5% antioxidant, 4% auxiliary agent, and the balance made up of rubber material.
[0088] The high molecular polymer is ethylene-vinyl acetate copolymer purchased from Guangzhou Hongcheng Plastic Chemical Co., Ltd. and sold as EVA1540 product.
[0089] The plasticizer is dioctyl phthalate.
[0090] The antioxidant is antioxidant 2246.
[0091] The auxiliary agents are dinitrosopentamethylenetetramine and zinc dibutyldithiocarbamate, and the mass ratio of the two is 2:1.
[0092] The rubber material is chloroprene rubber, which is purchased from Nippon Denka A-30 chloroprene rubber products.
[0093] The second aspect of the present embodiment provides a method for preparing the above-mentioned high-strength exterior wall insulation board, and the preparation method comprises the following steps: S1: mixing cement slurry, lightweight aggregate and additives to obtain a mixture; S2: adding the mixture to a slurry mixer and mixing with appropriate water for 1 hour, injecting the mixture into an insulation board mold, heating and calendering, and curing for 4 hours and drying the mixture until the moisture content is ≤1wt%.
[0094] Comparative Example 1
[0095] The specific implementation of this comparative example is basically the same as that of Example 1, except that the raw materials of the high-strength exterior wall insulation board, calculated by weight, include: 35 parts of cement slurry, 75 parts of lightweight aggregate, and 20 parts of additives.
[0096] Comparative Example 2
[0097] The specific implementation of this comparative example is basically the same as that of Example 1, except that the filling micropowder is modified xonotlite powder and modified perovskite powder; and the mass ratio of the modified xonotlite powder to the modified perovskite powder is 9:1.
[0098] Comparative Example 3
[0099] The specific implementation of this comparative example is basically the same as that of Example 1, except that the filling micropowder is modified xonotlite powder and modified perovskite powder; and the mass ratio of the modified xonotlite powder to the modified perovskite powder is 1:1.
[0100] Comparative Example 4
[0101] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the preparation method of modified xonotlite powder comprises the following steps, in parts by mass: S1: 12 parts of xonotlite powder are added to a reaction container, and 150 parts of deionized water are added for stirring and dispersion; S2: the temperature is raised to 85°C, 22 parts of 15wt% phosphoric acid aqueous solution are added, stirred evenly and kept warm for 2h to obtain a suspension of pretreated xonotlite powder; S3: 2 parts of metal salt, 1 part of sodium hydroxide and 0.5 parts of 3-aminopropyltriethoxysilane are added to the reaction container in sequence, mixed, cooled to 65°C and reacted for 3.5h, and the pH of the reaction system is maintained at 10; S4: after the reaction is completed, ethyl orthosilicate is added to the reaction container and stirred continuously, and the temperature is lowered to 55°C, and ultrasonically shaken at 500W for 2h, filtered, washed and dried after the reaction process to obtain modified xonotlite powder.
[0102] Comparative Example 5
[0103] The specific implementation method of this comparative example is basically the same as that of Example 1, with the only difference being: The preparation method of modified hard calcium silicate powder comprises the following steps, measured in parts by mass: S1: Take 12 parts of hard calcium silicate powder and add them into a reaction vessel, add 150 parts of deionized water and stir and disperse them; S2: Heat to 85°C, add 22 parts of 15wt% phosphoric acid aqueous solution, stir evenly and keep warm for 2h to obtain a suspension of pretreated hard calcium silicate powder; S3: Add ethyl orthosilicate to the reaction vessel and continue stirring, and cool to 55°C, react with 500W ultrasonic vibration for 2h, filter, wash and dry after the reaction process to obtain modified hard calcium silicate powder.
[0104] The amount of ethyl orthosilicate added is 10% of the mass of the S2 reaction solution system.
[0105] Comparative Example 6
[0106] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the preparation method of the modified perovskite powder comprises the following steps, in parts by mass: S1: adding 1.5 parts of perovskite powder to 50 parts of DMF solution prepared with 1 part of glutaric anhydride and 0.4 parts of 3-aminopropyltriethoxysilane, heating to 60°C and stirring for 3.5 hours, filtering and washing after completion to obtain the pretreated perovskite powder; S2: dissolving 3 parts of zinc acetate and 5 parts of 2-methylimidazole in 20 parts of methanol solvent respectively to prepare a solution, mixing the zinc acetate solution with 2 parts of the pretreated perovskite powder, heating to 80°C after mixing evenly, and dropping 2-methylimidazole solution under stirring at a speed of 800 r / min for 1.5 hours, adding 0.5 parts of triethylamine after the dropping is completed, then reducing the temperature to 65°C and keeping the temperature for reaction for 3 hours; S3: after the reaction is completed, centrifugation and filtration are performed to collect the solid product, which is then washed with methanol for multiple times and dried to obtain the product.
[0107] Comparative Example 7
[0108] The specific implementation of this comparative example is basically the same as that of Example 1, except that: the preparation method of the modified perovskite powder comprises the following steps, in parts by mass: S1: adding 3 parts of perovskite powder to 50 parts of DMF solution prepared with 1 part of glutaric anhydride and 0.4 parts of 3-aminopropyltriethoxysilane, heating to 60°C and stirring for 3.5 hours, filtering and washing after completion to obtain the pretreated perovskite powder; S2: dissolving 1 part of zinc acetate and 0.2 parts of 2-methylimidazole in 10 parts of methanol solvent to prepare a solution, mixing the zinc acetate solution with 2 parts of the pretreated perovskite powder, heating to 80°C and stirring at 800 r / min after mixing, and dropping 2-methylimidazole solution for 2 hours, adding 0.03 parts of triethylamine after the dropping is completed, and then reducing the temperature to 65°C and keeping the temperature for reaction for 5 hours; S3: after the reaction is completed, centrifugation and filtration are performed to collect the solid product, which is then washed with methanol for multiple times and dried to obtain the product.
[0109] Performance Evaluation
[0110] Thermal conductivity: The thermal conductivity performance test of the insulation boards prepared in all embodiments and comparative examples and stored in a normal warehouse for 1 month was carried out with reference to the method of GB / T 10294. The measured values were taken as the average value of 10 tests and recorded in Table 1.
[0111] Water absorption rate: Take the insulation board samples prepared in the embodiments and comparative examples, and make sure the surface is flat and without damage. Clean the surface of the sample to remove any dust or impurities, and allow it to dry naturally to constant weight under standard conditions (temperature 23±2°C, relative humidity 50±5%), and record the weight after drying (G). Completely immerse the dried sample in deionized water to ensure that all parts of the sample can fully contact the water. The immersion time is 48 hours. After the immersion is completed, carefully take out the sample, gently shake off excess water on the surface, avoid rubbing or squeezing the sample, and gently wipe off the water on the surface of the sample with a clean cloth, and then place it in a well-ventilated environment to dry naturally until the weight no longer changes. Record the weight at this time (B), calculate and record the water absorption during the period, water absorption % = (BG) / G × 100%, and take the average value of 10 tests as the measured value and record it in Table 1.
[0112] Weather resistance and UV resistance stability: 50 samples were prepared for the embodiments and comparative examples respectively, with a sample size of 5cm×5cm×2cm. The samples were first placed in a constant temperature and humidity chamber at 75°C and 100% humidity for 3 months. After being taken out, they were observed under a 200W ultraviolet lamp for 7 days to observe whether the insulation board samples showed obvious yellowing, surface oxidation damage, and wet rot. If so, they were recorded as unqualified, otherwise they were qualified. The results of the final sample qualification rate are calculated and recorded in Table 1.
[0113]
[0114] From the examples and comparative examples of the present application and the data results of Table 1, it can be known that examples 1 and 2 of the present application can be significantly better than comparative examples 1 to 7 in terms of thermal insulation performance, waterproof and moisture absorption resistance, weather resistance and UV resistance by adopting the technical solution defined in the present application. This is because the technical solution adopted in examples 1 and 2 can not only greatly increase the contact thermal resistance of the internal raw materials of the thermal insulation, but also form multiple surface pores and rough surfaces to reduce the effect of gas convection heat transfer; on the other hand, the addition of the modified filler can form a thin hydration layer on the surface during use, and the presence of the hydration layer makes it more difficult for external active molecules or corrosive substances to contact the thermal insulation board; and the modified particles can guide the aggregation of carriers and electron holes on the perovskite and zinc framework structures respectively under the illumination of the external wall thermal insulation board, thereby maintaining an extremely high surface light energy receiving capacity during the long-term use of the thermal insulation board, and consuming more energy during the long-term ultraviolet illumination process, thereby avoiding the phenomenon of oxidation yellowing and deterioration loss of the thermal insulation board.
Claims
1. A high-strength exterior wall insulation board, characterized in that: The raw materials include, by weight: 45-60 parts of cement slurry, 40-80 parts of lightweight aggregate, and 10-35 parts of additives; The cement slurry comprises, by weight percentage, 40-45% cement, 10-20% fly ash, 10-20% filler powder, and the balance made up of gypsum; The cement is at least one of ordinary Portland cement, sulphoaluminate cement and composite Portland cement; The fly ash is sodium-containing fly ash; The filler micropowder is modified xonotlite powder and modified perovskite powder; the mass ratio of the modified xonotlite powder to the modified perovskite powder is (3-5): (1-1.5); The preparation method of the modified xonotlite powder comprises the following steps: S1: adding xonotlite powder to a reaction container, adding deionized water for stirring and dispersing; S2: heating to 80-90°C, adding phosphoric acid aqueous solution, stirring evenly and keeping warm for 2-3 hours to obtain a suspension of pretreated xonotlite powder; S3: sequentially adding metal salt, alkali agent and silane coupling agent to the reaction container, mixing, cooling to 60-70°C for reaction for 3-4 hours, and maintaining the pH of the reaction system at 8-10; S4: adding ethyl orthosilicate to the reaction container after the reaction is completed, stirring continuously, cooling to 50-55°C, and reacting with 400-600W ultrasonic vibration for 1-2 hours, filtering, washing and drying after the reaction process to obtain the modified xonotlite powder; The mass ratio of the xonotlite powder to the phosphoric acid aqueous solution is (1-1.5):(2-3); The mass ratio of the xonotlite powder, the metal salt and the silane coupling agent is (1-1.5): (0.5-1): (0.1-0.2); The amount of ethyl orthosilicate added is 5-10% of the mass of the S3 reaction solution system; The preparation method of the modified perovskite powder comprises the following steps: S1: adding the perovskite powder to a DMF solution prepared with glutaric anhydride and a silane coupling agent, heating to 60-70° C., heating and stirring for 3-5 hours, filtering and washing after completion to obtain the pretreated perovskite powder; S2: dissolving zinc acetate and 2-methylimidazole in a methanol solvent to prepare a solution, mixing the zinc acetate solution with the pretreated perovskite powder, heating to 80-85° C. after mixing evenly, dripping the 2-methylimidazole solution under a stirring state of a speed of 60-120 r / min, the dripping time being 1-1.5 hours, adding triethylamine after the dripping is completed, then reducing the temperature to 60-75° C. and keeping the temperature for reaction for 3-4 hours; S3: centrifugally filtering after the reaction is completed, collecting the solid product, then washing with methanol for multiple times and drying to obtain the product; The average particle size of the perovskite powder is 400-600 nm; The mass ratio of the perovskite powder, glutaric anhydride and silane coupling agent is (1-2): (1-2): (0.3-0.5); The mass ratio of the pretreated perovskite powder, zinc acetate, 2-methylimidazole and triethylamine is (1.5-2): (0.1-0.5): (0.5-1.5): (0.01-0.05).
2. The high-strength exterior wall insulation board according to claim 1, characterized in that: The mass ratio of the cement slurry, lightweight aggregate and additive is (50-60):(55-70):(15-25).
3. The high-strength exterior wall insulation board according to claim 2, characterized in that: The lightweight aggregate comprises, by weight percentage, 80-90% hollow vitrified microspheres and 10-20% rice husk powder.
4. The high-strength exterior wall insulation board according to claim 3 is characterized in that: The average particle size of the hollow vitrified microspheres is 100 to 250 μm.
5. The high-strength exterior wall insulation board according to claim 4, characterized in that: The additives are calculated by mass percentage, and the raw materials include: 25-35% high molecular polymer, 0.5-1.5% stearic acid, 10-15% plasticizer, 0.1-1% antioxidant, 2-6% auxiliary agent, and the balance is made up of rubber material.
6. A method for preparing the high-strength exterior wall insulation board according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: S1: mixing cement slurry, lightweight aggregate and additives evenly to obtain a mixture; S2: adding the mixture into a slurry mixer and mixing with appropriate water for 0.5 to 1 hour, injecting the mixture into an insulation board mold, heating and calendering, curing for 3 to 5 hours, and drying the mixture until the moisture content is ≤1wt%.