A method for preparing a 355nm highly reflective thin film suitable for ultraviolet lasers

By replacing the traditional HfO2/SiO2 film stack with an irregular Al2O3/SiO2 film stack on the ultraviolet laser reflector, the multilayer film structure is optimized, the thin film damage problem under high power is solved, and a high laser damage threshold and low absorption loss of the high reflectivity thin film are achieved, which is suitable for high-power ultraviolet lasers.

CN118407004BActive Publication Date: 2026-11-17QILU ZHONGKE INST OF OPTICAL PHYSICS & ENG TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410553485.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-07
Publication Date
2026-11-17
Estimated Expiration
2044-05-07

AI Technical Summary

Technical Problem

Existing technologies make it difficult to fabricate 355nm high-reflectivity thin films with high laser damage thresholds, leading to film damage in ultraviolet lasers at high power, affecting the output power and beam quality of the laser, and resulting in high replacement costs.

Method used

An irregular Al2O3/SiO2 film stack shielded by an ion source is deposited on the outer layer of a regular HfO2/SiO2 film stack deposited with ion source assistance. This optimizes the composition and structure of the thin film material. The multilayer film system is deposited alternately by electron beam evaporation, which reduces secondary sputtering of outer layer deposited atoms and internal stress, thereby improving the resistance to laser damage.

Benefits of technology

It significantly improves the laser damage threshold of highly reflective films to 23.7 MW·cm⁻², reduces the absorption loss and internal stress of the films, and enhances the laser damage resistance of the films, making them suitable for high-power ultraviolet laser applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118407004B_ABST
    Figure CN118407004B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of optical thin films, specifically relating to a method for preparing a high-damage-threshold 355nm high-reflectivity thin film for ultraviolet laser mirrors. First, a regular 1 / 4 wavelength thickness HfO2 layer and SiO2 layer with 15 cycles of deposition is assisted by plasma generated by an ion source. Then, an outer layer film system of 0.8Al2O3, 1.2SiO2, 0.8Al2O3, 1.2SiO2, 0.8Al2O3, 1.2SiO2, and 0.8Al2O3 is deposited while shielding the ion source. A three-material dual-film stack system is used; the HfO2 / SiO2 stack effectively ensures a reflectivity greater than 99.5% for the high-reflectivity film. Depositing an irregular Al2O3 / SiO2 film stack ending in Al2O3 on the outer layer while shielding the ion source effectively improves the outer layer structure, reduces the outer electric field strength and internal stress of the film, reduces absorption loss, and further improves the laser damage threshold of the high-reflectivity film to 23.7 MW·cm. ‑2 The preparation method is efficient and easy to implement, significantly improves the laser damage resistance of the thin film, is reproducible, and is suitable for industrial production. It has great market potential in the field of high-power ultraviolet lasers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of optical thin films, specifically relating to a method for preparing a high-damage-threshold 355nm high-reflectivity thin film for ultraviolet laser mirrors. By depositing an irregular Al2O3 / SiO2 film stack ending in Al2O3 to shield the ion source on the outer layer of a regular HfO2 / SiO2 film stack deposited with ion source assistance, the laser damage resistance performance can be effectively improved. Background Technology

[0002] Lasers are one of the four great inventions of human technology in the 20th century. According to statistics, the overall market size of lasers in my country reached 91.8 billion yuan in 2022. The optical coating lenses required for lasers and laser processing equipment exceeded 3 billion yuan per year. At the same time, the application rate of lasers in manufacturing is only 30%. Laser-related industries have broad market prospects in my country's industrial system.

[0003] Ultraviolet (UV) lasers generate short-wavelength lasers that are easily focused and can directly break chemical bonds in matter. They are often used to process materials that infrared and visible lasers cannot, and are widely used in the ultra-precision machining of materials such as semiconductors, ceramics, and copper alloys. Applications include drilling and cutting flexible circuit boards, scribing sapphire substrates for LEDs, cutting solar panels, and marking medical devices. Optical thin films are a key component of UV lasers, playing a crucial role in laser generation, transmission, modulation, and synthesis. For UV laser mirror elements, the reflectivity and laser damage resistance of highly reflective thin films are key factors affecting laser output power and beam quality. Currently, the high-end thin-film products required for domestically produced high-power ultraviolet lasers mainly rely on imports. As for ultraviolet ultrafast lasers, domestically produced ones are mainly low-power products under 50W, accounting for more than 50% of sales in my country, but the unit price is relatively low. Imported ultraviolet ultrafast lasers are equipped with high-end thin-film products, which are mostly high-power products with high unit prices. Their sales volume is only 40%, but they take away nearly 70% of the sales revenue. The slow development of domestic thin-film technology has become one of the main bottlenecks restricting the development of high-power lasers.

[0004] Currently, the main method for depositing 355nm high reflectivity thin films in China is to use ion source-assisted alternating deposition of regular 1 / 4 wavelength thickness hafnium oxide (HfO2) and silicon oxide (SiO2). The thin films prepared by this method have high reflectivity, but with the increase of ultraviolet laser power, there are three main problems: (1) Due to the narrow band gap of HfO2 material, electrons in the film in equilibrium state are prone to reach the excited state after absorbing photons, and break free from atomic binding, resulting in damage to the film structure; (2) Under ion source-assisted deposition, the bombardment of charged ions in the source gas will cause secondary sputtering of deposited atoms, resulting in increased micro-defect density and increased internal stress of the film; (3) Regular film systems ending with low refractive index material SiO2 have a high electric field intensity in the outer layer, and the absorption loss of the outer layer of the film is large. All of the above defects can cause a decline in the laser damage threshold of thin films. After laser irradiation, the material absorbs laser energy, leading to changes in its microscopic state. At low laser power, these changes are difficult to translate into macroscopic damage. However, when the laser power reaches a certain level, the laser can cause material breakdown, melting, vaporization, etc., ultimately resulting in irreversible damage to the laser-irradiated area, making it unable to withstand the operation of high-power lasers. Once optical thin-film components are damaged, they are difficult to completely repair, and replacement costs are high, maintenance cycles are long, ultimately leading to irreparable losses.

[0005] In summary, the traditional methods for depositing 355nm high reflectivity films are limited by their film structure, material band gap, and ion source process, making it difficult to obtain 355nm high reflectivity films with high laser damage thresholds for ultraviolet lasers. Summary of the Invention

[0006] The purpose of this invention is to overcome the shortcomings of existing technologies and provide a method for preparing a high-damage-threshold 355nm high-reflectivity thin film for ultraviolet laser mirrors. By adding an irregular Al2O3 / SiO2 film stack ending in Al2O3 to the outer layer of a regular HfO2 / SiO2 film stack deposited with ion source assistance to shield the ion source, the laser damage resistance performance can be effectively improved.

[0007] To achieve the above objectives, this invention provides a method for preparing a high-damage-threshold 355nm high-reflectivity thin film for ultraviolet laser mirrors. From the perspective of optimizing the composition of the coating material and the outer layer structure of the thin film, firstly, plasma generated by an ion source is used to assist in the deposition of a regular 1 / 4 wavelength thickness HfO2 layer and SiO2 layer with 15 cycles. Then, the ion source is shielded to continue deposition of an outer layer film system of 0.8Al2O3, 1.2SiO2, 0.8Al2O3, 1.2SiO2, 0.8Al2O3, 1.2SiO2, 0.8Al2O3, 1.2SiO2, and 0.8Al2O3. The specific deposition steps are as follows: (1) Clean the substrate and load it into the coating machine. The substrate is made of quartz. (2) Control the vacuum level in the coating machine chamber to reach 9.0×10-4 Once the substrate temperature stabilizes at 210℃, the ion source is activated to pre-clean the substrate coating surface for 6 minutes. (3) With the assistance of an ion source, HfO2 and SiO2 layers with a regular 1 / 4 wavelength thickness of 15 cycles are alternately deposited by electron beam evaporation; (4) Open the ion source shielding baffle and use electron beam evaporation to deposit 0.8Al2O3, 1.2SiO2, 0.8Al2O3, 1.2SiO2, 0.8Al2O3, 1.2SiO2, and 0.8Al2O3 in sequence. There are a total of 7 outer film systems, where 0.8 and 1.2 represent multiples of the regular 1 / 4 wavelength optical thickness. (5) After the deposition is completed, there are a total of 37 layers of ultraviolet high reflective film. The film system is SUB[(HL)15(0.8a1.2l)30.8a]AIR, where H and L are HfO2 and SiO2 deposited by ion source assistance, respectively, and a and l are Al2O3 and SiO2 deposited by shielding ion source, respectively. SUB is a quartz substrate and AIR is an air atmosphere. After the system cools down, the substrate with high reflective film is taken out.

[0008] The substrate is a quartz mirror.

[0009] In step (4) of this invention, the ion source shielding baffle is opened to block the plasma generated by the source gas, reduce the secondary sputtering of atoms deposited on the outer layer of the thin film, reduce the internal stress of the outer film layer, and keep the ion source gas charge constant to maintain the stability of the vacuum chamber environment. In steps (3) and (4), the ion source anode voltage, anode current and neutralizer current parameters of the three materials HfO2, Al2O3 and SiO2 are respectively: HfO2: 170V, 5A, 300MA, Al2O3 and SiO2: 150V, 2A, 200MA; the source oxygen charge of the three materials HfO2, Al2O3 and SiO2 is 24sccm, 15sccm and 14sccm.

[0010] The present invention also provides a high-damage-threshold 355nm high-reflectivity thin film for ultraviolet laser mirrors prepared by the above method.

[0011] This invention addresses the problem of laser damage to the outer layer of thin films by employing an irregular Al2O3 / SiO2 film stack with a shielded ion source instead of the traditional HfO2 / SiO2 film stack in the outer layer of a high-reflectivity thin film. The band gap of Al2O3 is 8.8 eV, greater than that of HfO2 (5.6 eV). When a certain amount of laser energy is applied to the film, only a small number of shallow-level electrons in the outer Al2O3 / SiO2 film stack are excited to the conduction band, and their accumulation density is insufficient to cause damage. After laser irradiation, these electrons decay back to deeper energy levels. Furthermore, with the shielded ion source, the coating vacuum environment is stable, the crystallinity of the Al2O3 / SiO2 outer film layer decreases, internal stress is low, and it exhibits amorphous properties, acting as a buffer layer. This significantly improves the laser damage threshold of the thin film; the laser damage threshold of the high-reflectivity film of this invention reaches 23.7 MW·cm⁻¹. -2 .

[0012] Compared with existing technologies, this invention employs a three-material dual-film stack system. The HfO2 / SiO2 film stack effectively ensures that the high-reflectivity film has a reflectivity greater than 99.5%, meeting the reflectivity requirements of ultraviolet laser mirrors. The outer layer, coated with an irregular Al2O3 / SiO2 film stack ending in Al2O3 to shield the ion source, effectively improves the outer layer structure, reduces the outer electric field strength and internal stress of the film, lowers absorption loss, and further increases the laser damage threshold of the high-reflectivity film to 23.7 MW·cm⁻¹. -2 This thin film preparation method is efficient and easy to implement, significantly improves the laser damage resistance of the thin film, is reproducible, and is suitable for industrial production. It helps reduce the dependence of the domestic ultraviolet laser industry on imported high-end thin film products and has great market prospects in the field of high-power ultraviolet lasers. Attached Figure Description

[0013] Figure 1 This is a schematic diagram showing the performance test results of the highly reflective thin film prepared in Example 1 of the present invention. Detailed Implementation

[0014] The present invention will be further described in detail below with reference to specific embodiments and accompanying drawings.

[0015] Example 1: This embodiment relates to a method for preparing a high-damage-threshold 355nm high-reflectivity thin film for ultraviolet laser mirrors, the specific steps of which are as follows: (1) Clean the uncoated ultraviolet laser mirror with alcohol, acetone and lint-free cloth. The mirror has a diameter of 25mm and a thickness of 5mm. Then fix the mirror on the workpiece tray and put it into the coating machine. Evacuate the air and heat the mirror. The heating temperature is set to 210℃. (2) When the vacuum degree in the coating machine chamber reaches 9.0×10-4 When the temperature of the reflector substrate is heated to 210℃, wait for the system to stabilize for 30 minutes, turn on the ion source power supply for pre-cleaning for 6 minutes. The ion source pre-cleaning anode voltage, anode current and neutralizer current are 120V, 2A, 200MA, and the oxygen charge is 10sccm.

[0016] (3) After cleaning, HfO2 and SiO2 layers with a regular 1 / 4 wavelength thickness are deposited alternately for 15 cycles using electron beam evaporation and ion source assistance. That is, HfO2 is deposited as the first layer, SiO2 is deposited as the second layer, and HfO2 and SiO2 are deposited alternately for a total of 30 layers. The wavelength is 355nm ultraviolet. After the 30th SiO2 layer is deposited, the ion source shielding baffle is opened to block the charged plasma bombardment of the ion source. The source gas charge remains unchanged. Electron beam evaporation is used to deposit the outer film system of 0.8Al2O3, 1.2SiO2, 0.8Al2O3, 1.2SiO2, 0.8Al2O3, 1.2SiO2, and 0.8Al2O3 in sequence. Among them, 0.8 and 1.2 represent multiples of the regular 1 / 4 wavelength optical thickness. The deposition conditions of the thin film material are shown in Table 1.

[0017] Table 1 Deposition conditions for thin film materials Material Deposition rate (nm / s) Electron gun oxygen flux (sccm) <![CDATA[Oxygen partial pressure (×10 -2 Pa)]]> Anode voltage (V) Anode current (A) Neutralizer current (mA) Source oxygen flux (sccm) <![CDATA[HfO2]]> 0.15 25 2.0 170 5 300 24 <![CDATA[Al2O3]]> 0.3 5 2.0 150 2 200 15 <![CDATA[SiO2]]> 0.4 0 1.6 150 2 200 14 (4) After the outer layer film is deposited, there are a total of 37 high-reflectivity thin films, and the film system is SUB[(HL)]. 15 (0.8a1.2l) 3 0.8a]AIR, where H and L are HfO2 and SiO2 deposited with ion source assistance, respectively, a and l are Al2O3 and SiO2 deposited with shielded ion source, respectively, SUB is a quartz substrate, and AIR is an air atmosphere; turn off the heating and ion source power supply, wait for the system to cool down naturally to room temperature, and the system vacuum degree to return to atmospheric pressure, and take out the mirror with the high reflectivity film deposited.

[0018] Example 2: This embodiment tests the performance of the high-reflectivity thin film deposited on the mirror in Example 1. Spectroscopic measurements were performed using a Lamda 950 spectrometer from PE Corporation (USA). This instrument has a measurement range of 175-3300 nm, a resolution of no more than 0.05 nm in the ultraviolet band, and a wavelength accuracy of up to 0.08 nm. The test results are as follows: Figure 1 As shown, the high reflectivity of the high reflectivity film at 355nm is greater than 99.5%.

[0019] A laser with a power of 12W, a wavelength of 355nm, a frequency of 70kHz, and a pulse width of approximately 15ns was used to irradiate 10 fixed test points on the highly reflective film deposited in Example 1. Damage spots were observed using an optical microscope. The maximum peak power density that the highly reflective film could withstand was used as the laser damage threshold. The laser damage threshold of the highly reflective film deposited in Example 1 was 23.7MW·cm⁻¹. -2 .

[0020] Using the same laser damage threshold testing method, high-reflectivity thin films with an existing outer plasma-assisted process were tested. The film system was SUB[(HL)]. 18 ]AIR and SUB[(HL) 15 (AL) 3 AIR, whose laser damage threshold is 3MW·cm -2 and 14MW·cm -2 In summary, through the improvement of plasma processing and optimization of the film system in this invention, the laser damage threshold of the 355nm high-reflectivity thin film deposited by this invention is significantly improved.

Claims

1. A method for preparing a high-damage-threshold 355 nm high-reflectance thin film for an ultraviolet laser mirror, characterized in that, First, plasma-assisted deposition of 15 cycles of regular 1 / 4 wavelength thickness HfO2 and SiO2 layers was performed. Then, the ion source was shielded to continue deposition of an outer film system of 0.8Al2O3, 1.2SiO2, 0.8Al2O3, 1.2SiO2, 0.8Al2O3, 1.2SiO2, 0.8Al2O3, 1.2SiO2, and 0.8Al2O3. The specific deposition steps are as follows: (1) Clean the substrate and load it into the coating machine; (2) Control the vacuum level in the coating machine chamber, stabilize the substrate temperature at 210℃, and start the ion source to pre-clean the substrate coating surface for 6 minutes; (3) With the assistance of an ion source, HfO2 and SiO2 layers with a regular 1 / 4 wavelength thickness of 15 cycles are alternately deposited by electron beam evaporation; (4) Open the ion source shielding baffle to block the plasma generated by the source gas. Keep the source gas charge constant to maintain the stability of the vacuum chamber environment. Use electron beam evaporation to deposit 0.8Al2O3, 1.2SiO2, 0.8Al2O3, 1.2SiO2, 0.8Al2O3, 1.2SiO2, 0.8Al2O3, 1.2SiO2, and 0.8Al2O3 in sequence. There are a total of 7 outer film systems. Among them, 0.8 and 1.2 represent multiples of the regular 1 / 4 wavelength optical thickness. (5) After the coating is completed, there are a total of 37 layers of high reflectivity film. After the system cools down, the substrate coated with high reflectivity film is taken out.

2. The method for preparing a high-damage-threshold 355nm high-reflectivity thin film for ultraviolet laser mirrors according to claim 1, characterized in that, The substrate is a quartz mirror.

3. The method for preparing a high-damage-threshold 355nm high-reflectivity thin film for ultraviolet laser mirrors according to claim 1, characterized in that, In steps (3) and (4), the ion source anode voltage, anode current, and neutralizer current parameters for the three materials are as follows: HfO2: 170V, 5A, 300mA; Al2O3 and SiO2: 150V, 2A, 200mA; and the source oxygen charge for the three materials HfO2, Al2O3, and SiO2 is 24sccm, 15sccm, and 14sccm, respectively.

4. The method for preparing a high-damage-threshold 355nm high-reflectivity thin film for ultraviolet laser mirrors according to claim 1, characterized in that, Step (2) The anode voltage, anode current and neutralizer current for the ion source pre-cleaning are 120V, 2A and 200mA, and the oxygen charge is 10sccm.

5. The method for preparing a high-damage-threshold 355nm high-reflectivity thin film for ultraviolet laser mirrors according to claim 1, characterized in that, The wavelengths described in steps (3) and (4) are ultraviolet 355nm.

6. A high-damage-threshold, 355nm high-reflectivity thin film for ultraviolet laser mirrors prepared by the method of claim 1, characterized in that, UV high reflectance thin film 37 layers, film system is SUB[(HL) 15 (0.8a1.2l)30.8a]AIR, wherein H and L are HfO2 and SiO2 deposited by ion source assisted deposition, respectively, a and l are Al2O3 and SiO2 deposited by shadowing ion source, respectively, SUB is a quartz substrate, and AIR is an air atmosphere.

7. The high-damage-threshold 355nm high-reflectivity thin film for ultraviolet laser mirrors according to claim 6, characterized in that, The laser damage threshold is 23.7 MW-cm -2 .

Citation Information

Patent Citations

  • Method for preparing HfO2 / SiO2 multi-layer reflective film by electronic beams

    CN101713061A

  • Plating method for improving damage threshold of 355nm high-reflective film

    CN103215551A

  • Reflection mirror for laser

    JP1997222507A

  • Multilayer film mirror

    JP2015079132A