A preparation method of biomass porous carbon for supercapacitor and supercapacitor

By assisting hydrothermal pre-carbonization and pyrolytic carbonization by pyridinethiourea hydrochloride, high porosity and high doping amount of biomass porous carbon are generated, which solves the problem of the existing biomass porous carbon materials with lower capacitance and insufficient cycle stability. Problem, high specific capacitance and excellent cycle stability of supercapacitors are achieved.

CN118419927BActive Publication Date: 2024-12-03FUJIAN XINSEN CARBON
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410688798.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-30
Publication Date
2024-12-03
Estimated Expiration
2044-05-30

AI Technical Summary

Technical Problem

The existing biomass porous carbon materials have a small specific surface area, irregular pore structure, and small doped atom content, resulting in low specific capacitance and insufficient cycling stability, which cannot meet the high energy density and power density requirements of supercapacitors.

Method used

Pyridinethiourea hydrochloride is used as an auxiliary agent for hydrothermal pre-carbonization and pyrolytic carbonization. Through the hydrothermal process, hydrothermal carbon with pore structure is generated, and C-S and C-N bonds are formed at high temperatures. , improve specific surface area and porosity, and act as an activator and heteroatom dopant to enhance the electrochemical properties of porous carbon.

Benefits of technology

The prepared biomass porous carbon has a high specific surface area, high microporosity, and high nitrogen and sulfur doping, which significantly improves the specific capacity and cycling stability of the supercapacitor, and can maintain high capacitance under high current density. And the capacity retention rate is as high as 89% after 5000 cycles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118419927B_ABST
    Figure CN118419927B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing a porous biomass carbon for supercapacitor and a supercapacitor. The method for preparing the porous biomass carbon comprises the following steps: pretreatment, hydrothermal precarbonization, pyrolysis carbonization, and deoxidation treatment. The present invention uses pyridinethiourea hydrochloride as an auxiliary agent to hydrothermally precarbonize biomass, and then pyrolysis carbonization and deoxidation treatment to obtain the porous biomass carbon; pyridinethiourea hydrochloride is both an auxiliary agent for hydrothermal precarbonization and an activator and heteroatom dopant for pyrolysis carbonization; the specific surface area of ​​the prepared porous biomass carbon reaches 1800m 2 / g or more, microporosity of more than 86%, nitrogen content of more than 7%, sulfur content of more than 4%, oxygen content of less than 1.5%. The prepared biomass porous carbon has high specific capacitance and excellent cycle stability when used as an electrode material for supercapacitors.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of supercapacitor electrode materials, and in particular relates to a method for preparing biomass porous carbon for supercapacitors and a supercapacitor. Background Art

[0002] Supercapacitors, also known as double-layer capacitors, store energy by polarizing electrolytes with an external electric field, so that the charged ions in the electrolyte form double layers on the surfaces of electrodes with opposite charges. The energy storage process is a physical process, and the process is completely reversible, which is different from the electrochemical energy storage process of batteries. Supercapacitors have both the energy storage characteristics of batteries and the characteristics of capacitors that can be charged and discharged quickly. They are expected to replace lithium batteries and ordinary supercapacitors as a new type of energy storage device. As a new type of energy storage device, supercapacitors have become the first choice in the field of fast and high-power energy storage systems with their high energy density and power density and excellent cycle performance. They have important application value in portable instruments, hybrid vehicle power supplies, information technology and other fields.

[0003] One of the key factors that determine the performance of supercapacitors is the performance of electrode materials. Biomass porous carbon materials have been studied as promising electrode materials for supercapacitors. According to existing reports, mesopores with pore sizes between 2 and 50 nm not only allow electrolyte ions to pass quickly and provide an effective interface for contact with electrolyte ions, but also serve as channels for electrolyte ions to penetrate into micropores. Therefore, the development of porous carbon with interconnected macropores, mesopores and micropores and a high atomic doping content plays an important role in enhancing its electrochemical properties as an active material for supercapacitor electrodes. Limited by the structural characteristics of biomass itself, biomass porous carbon usually has an irregular pore structure, a small specific surface area, and a low content of doped atoms, so the specific capacity is low and cannot meet actual requirements.

[0004] Chinese patent CN104803383A discloses a method for preparing supercapacitor activated carbon using camphor leaves. The method uses camphor leaves as raw materials and is obtained through water washing, drying, acid leaching, carbonization, acid washing, and drying. The specific surface area of ​​the obtained activated carbon is 963.70 to 1424.19 m 2 / g, and its specific capacity can reach 95-120F / g at a discharge current of 300mA. This method realizes the collection and utilization of camphor leaves, avoids the pollution caused by incineration, and realizes the effective utilization of resources. However, the prepared porous carbon material has a low specific surface area and a low specific capacitance.

[0005] Chinese patent CN110526243A discloses a method for preparing biomass porous carbon for supercapacitors and its application, which belongs to the field of supercapacitor electrode material preparation. It uses monk fruit shell as a carbon source, KOH and urea as activators, and adopts a high-temperature carbonization method to prepare an aqueous supercapacitor electrode material with excellent performance. The inventive method has a simple, reliable, and green production process, but the specific capacitance of the prepared porous carbon is low. At a current density of 1A / g, the specific capacitance is only 171F / g. Summary of the invention

[0006] In view of the above problems, the purpose of the present invention is to provide a method for preparing biomass porous carbon for supercapacitors. The prepared porous carbon has high porosity and specific surface area, and has a high doping amount of nitrogen and sulfur atoms; the porous carbon is used as an electrode material in supercapacitors to improve specific capacitance and cycle stability.

[0007] The present invention provides the following technical solutions to solve the above technical problems:

[0008] A method for preparing biomass porous carbon for supercapacitor comprises the following steps:

[0009] (S1) pretreatment: crushing, washing and drying the biomass raw materials in sequence to obtain pretreated biomass;

[0010] (S2) hydrothermal pre-carbonization: adding the pretreated biomass and pyridinethiourea hydrochloride in a mass ratio of 100:(15-25) to water, heating and heat preservation in a sealed environment, cooling to room temperature after heat preservation, filtering and drying to obtain a solid substance, i.e., hydrothermal charcoal;

[0011] (S3) pyrolysis carbonization: mixing the hydrothermal carbon and the inorganic base in a mass ratio of 100:(30-50), carbonizing under an inert atmosphere, and then cooling, washing, and drying to obtain pyrolysis carbon;

[0012] (S4) Deoxidation treatment: placing the pyrolytic carbon in an atmosphere of hydrogen and nitrogen mixed gas at 900-1100° C., and then cooling and grinding to obtain biomass porous carbon for supercapacitor.

[0013] The present invention uses pyridinethiourea hydrochloride as an auxiliary agent to hydrothermally pre-carbonize biomass. During the hydrothermal process, the biomass carbon skeleton is depolymerized and reorganized, and various oxygen-containing structures (including cross-linking bonds, functional groups and heterocycles) are removed to produce hydrothermal carbon with a porous structure. The addition of pyridinethiourea hydrochloride enhances the deoxidation ability of hydrothermal carbon. The possible reason is that the pyridine ring of the large π bond in pyridinethiourea hydrochloride can interact with the large π bond of the benzene ring of the biomass, and pyridinethiourea hydrochloride has good solubility for biomass raw materials, which promotes the hydrothermal carbonization reaction. In the subsequent pyrolysis carbonization stage, pyridinethiourea hydrochloride decomposes at high temperature to generate ammonia and carbon dioxide, thereby increasing the porosity of the carbon, that is, pyridinethiourea hydrochloride plays the role of an activator in the pyrolysis carbonization stage. In addition, the activator inorganic base has a strong dehydration and intercalation effect, which is conducive to the hydrothermal carbon to produce a large number of pore structures, which can greatly increase its specific surface area. However, the amount of inorganic base added during the activation process is often large, and the introduction of pyridinethiourea hydrochloride in the present invention allows the hydrothermal carbon to be pyrolyzed and carbonized under the condition of adding a small amount of activator inorganic base (only 30% to 50% of the mass of the hydrothermal carbon raw material). A large number of pore structures can be formed during the pyrolysis and carbonization of the hydrothermal carbon; rich pore structures and high specific surface area can improve the specific capacity and cycle stability of porous carbon as an electrode material. At the same time, pyridinethiourea hydrochloride is also a nitrogen source and a sulfur source. Under high temperature conditions, sulfur and nitrogen react with carbon in porous carbon respectively to form CS bonds and CN bonds, realizing heteroatom doping; nitrogen and sulfur doping can improve the wettability of the porous carbon surface, further improving the specific capacity of porous carbon as an electrode material.

[0014] In summary, the present invention uses pyridinethiourea hydrochloride to pre-carbonize biomass, which is not only an auxiliary agent for hydrothermal pre-carbonization, but also an activator and heteroatom dopant for subsequent pyrolysis carbonization, and plays a multi-functional role.

[0015] Furthermore, the biomass in step (S1) is at least one of coconut shell, palm shell, walnut shell and apricot shell; the crushing is to crush to 100-400 mesh, and the crushing method adopts air flow crushing, high-speed crushing or ball milling.

[0016] Furthermore, the pyridinethiourea hydrochloride in step (S2) is at least one of 2-pyridinethiourea hydrochloride, 3-pyridinethiourea hydrochloride, 4-pyridinethiourea hydrochloride, and pyridinethione urea; preferably 4-pyridinethiourea hydrochloride.

[0017] Furthermore, the pyridinethiourea hydrochloride is obtained by a preparation method comprising the following steps: dissolving pyridinethiourea in a solvent and adding hydrochloric acid; stirring the solution and heating it under reflux for 4 to 6 hours; filtering after the reaction, washing with water, and drying to obtain pyridinethiourea hydrochloride.

[0018] Furthermore, in step (S2), the solid-liquid ratio of the total mass of the pretreated biomass and pyridinethiourea hydrochloride to water is 1g:3-5mL.

[0019] Furthermore, the heating and heat preservation treatment in step (S2) is carried out at 180-250° C. for 3-5 hours; and the drying is carried out in a blast dryer at 80-120° C. for 24-48 hours.

[0020] After hydrothermal pre-carbonization, the biomass forms hydrothermal carbon with a porous structure, and pyridinethiourea hydrochloride is retained in the hydrothermal carbon and continues to participate in the reaction in the subsequent pyrolysis carbonization process.

[0021] Furthermore, the inorganic base in step (S3) is KOH and / or NaOH.

[0022] Furthermore, the carbonization conditions of step (S3) are: under an inert atmosphere, heating to 500-700°C at a heating rate of 3-8°C / min, and keeping warm for 2-4h; then heating to 800-900°C and keeping warm for 1-3h; the inert atmosphere is an oxygen content below 1%, such as a nitrogen or argon atmosphere.

[0023] During the pyrolysis carbonization process, gradient carbonization is adopted, which is beneficial to improving the porosity of porous carbon and the effective doping of nitrogen and sulfur.

[0024] Furthermore, the water washing in step (S3) is washing with deionized water until neutral; and the drying is drying in an oven at 80-120° C. for 24-36 hours.

[0025] Furthermore, in step (S4), the volume fraction of hydrogen in the hydrogen-nitrogen mixed gas is 4% to 7%, and the reaction time is 0.5 to 2 hours.

[0026] The pyrolytic carbon formed after pyrolysis carbonization under the action of the activating agent inorganic base has oxygen-containing groups on its surface. Although the presence of oxygen-containing groups can increase the capacitance, the oxygen-containing groups have strong electrochemical activity and are prone to decomposition reactions during charging and discharging, which can easily lead to a decrease in the cycle stability of the supercapacitor. Therefore, in the present invention, hydrogen is used for high-temperature thermal reduction after pyrolysis carbonization to remove the oxygen-containing groups on the surface of the pyrolytic carbon.

[0027] Furthermore, the grinding in step (S4) is performed by a jet mill, and the particle size D50 after grinding is 6 to 10 μm.

[0028] The present invention also provides a supercapacitor, whose electrode comprises a current collector and an active material layer attached to the surface of the current collector, and the active material layer comprises the biomass porous carbon prepared by the above preparation method.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] (1) The present invention uses pyridinethiourea hydrochloride as an auxiliary agent to hydrothermally pre-carbonize biomass, and then performs pyrolysis carbonization and deoxidation treatment to prepare biomass porous carbon for supercapacitor. Pyridinethiourea hydrochloride is not only an auxiliary agent for hydrothermal pre-carbonization, but also an activator and heteroatom dopant for pyrolysis carbonization. The specific surface area of ​​the biomass porous carbon prepared by the preparation method of the present invention is 1800m 2 / g or more, the microporosity is more than 86%, the nitrogen content is more than 7%, the sulfur content is more than 4%, and the oxygen content is less than 1.5%.

[0031] (2) The present invention prepares biomass porous carbon containing a large amount of pore structure under the condition of adding a small amount of activator inorganic base (only 30% to 50% of the mass of the hydrothermal carbon raw material).

[0032] (3) The biomass porous carbon prepared by the present invention has high specific capacitance and excellent cycle stability when used as an electrode material for supercapacitors. The specific capacitance of the supercapacitor is above 280 F / g at a current density of 1 A / g, and can still reach above 180 F / g at a high current density of 30 A / g. The capacitance retention rate after 5000 cycles at a current density of 5 A / g is as high as over 89%. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is the SEM image of the biomass porous carbon prepared in Example 1. DETAILED DESCRIPTION

[0034] The present invention will be further described below in conjunction with specific examples. Unless otherwise specified, the "parts" described in the examples of the present invention are all parts by weight. The reagents used are all commercially available reagents in the art.

[0035] Pyrithione urea was selected from Wuhan Pushida Biotechnology Co., Ltd. with a purity of 99%.

[0036] Preparation of pyridinethiocarbamide hydrochloride

[0037] Preparation Example 1

[0038] Dissolve 100 g of 2-pyridinethiourea in anhydrous acetonitrile, add 240 g of 12 wt% hydrochloric acid; stir and heat the solution to 50° C., and reflux for 5 h; after the reaction is completed, filter, wash with water, and dry to obtain 2-pyridinethiourea hydrochloride.

[0039] Preparation Example 2

[0040] Dissolve 100 g of 4-pyridinethiourea in anhydrous acetonitrile, add 240 g of 12 wt% hydrochloric acid; stir and heat the solution to 50° C., and reflux for 5 h; after the reaction is completed, filter, wash with water, and dry to obtain 4-pyridinethiourea hydrochloride.

[0041] Example 1

[0042] Biomass porous carbon for supercapacitors comprises the following steps:

[0043] (S1) pretreatment: crushing the coconut shell to 200 meshes by air flow crushing, then washing and drying to obtain pretreated biomass;

[0044] (S2) Hydrothermal pre-carbonization: 200 g of the pretreated biomass and 30 g of 2-pyridylthiourea hydrochloride prepared in Preparation Example 1 were added to 800 mL of pure water, sealed in a hydrothermal kettle and kept at 220° C. for 4 h. After the heat preservation, the mixture was cooled to room temperature, filtered, and dried in a blast dryer at 100° C. for 48 h to obtain a solid substance, i.e., hydrothermal charcoal.

[0045] (S3) Pyrolysis carbonization: 100 g of hydrothermal charcoal was mixed with 30 g of NaOH and placed in a rotary kiln with a rotation speed of 20 rpm. The temperature was raised to 600° C. at a heating rate of 6° C. / min under an argon atmosphere and kept at that temperature for 3 h; the temperature was then raised to 850° C. at a heating rate of 6° C. / min and kept at that temperature for 2 h; after the heat preservation, the mixture was cooled to room temperature, washed with water three times until neutral, and dried in an oven at 100° C. for 24 h to obtain pyrolytic charcoal;

[0046] (S4) Deoxidation treatment: The pyrolytic carbon was placed in a horizontal induction furnace, and a hydrogen-nitrogen mixed gas with a hydrogen content of 5 vol% was introduced. The temperature was raised to 900°C at a heating rate of 8°C / min, and the temperature was kept for 1 hour. Then, the carbon was cooled and ground to obtain a biomass porous carbon with a particle size D50 of 6.8 μm. The SEM image of the carbon is shown in FIG. Figure 1 shown.

[0047] Example 2

[0048] The rest is the same as Example 1, except that pyrithione urea is used in step (S2) instead of 2-pyrithione urea hydrochloride, and finally a biomass porous carbon with a particle size D50 of 7.2 μm is obtained.

[0049] Example 3

[0050] The rest is the same as Example 1, except that in step (S2), 4-pyridinethiourea hydrochloride prepared in Preparation Example 2 is used instead of 2-pyridinethiourea hydrochloride, and finally a biomass porous carbon with a particle size D50 of 7.1 μm is obtained.

[0051] Example 4

[0052] The rest is the same as Example 3, except that KOH is used instead of NaOH in step (S3), and finally a biomass porous carbon with a particle size D50 of 7.4 μm is obtained.

[0053] Example 5

[0054] The rest is the same as Example 4, except that the raw materials in step (S2) are: 200 g of pretreated biomass and 36 g of 4-pyridinethiourea hydrochloride, and finally a biomass porous carbon with a particle size D50 of 6.9 μm is obtained.

[0055] Example 6

[0056] The rest is the same as Example 4, except that the raw materials in step (S2) are: 200 g of pretreated biomass and 42 g of 4-pyridinethiourea hydrochloride, and finally a biomass porous carbon with a particle size D50 of 7.5 μm is obtained.

[0057] Example 7

[0058] The rest is the same as Example 4, except that the raw materials in step (S2) are: 200 g of pretreated biomass and 50 g of 4-pyridinethiourea hydrochloride, and finally a biomass porous carbon with a particle size D50 of 7.3 μm is obtained.

[0059] Example 8

[0060] The rest is the same as Example 4, except that the raw materials in step (S3) are: 100g hydrothermal charcoal and 50g KOH, and finally a biomass porous charcoal with a particle size D50 of 7.1μm is obtained.

[0061] Example 9

[0062] The rest is the same as Example 1, except that walnut shells are used instead of coconut shells in step (S1), and finally a biomass porous carbon with a particle size D50 of 7.2 μm is obtained.

[0063] Comparative Example 1

[0064] The rest is the same as Example 1, except that 2-pyridinethiourea hydrochloride is not used in step (S2), and finally a biomass porous carbon with a particle size D50 of 7.6 μm is obtained.

[0065] Comparative Example 2

[0066] The rest is the same as Example 1, except that thiourea is used in step (S2) instead of 2-pyridinethiourea salt, and the acid salt finally produces biomass porous carbon with a particle size D50 of 7.5 μm.

[0067] Application Example 1

[0068] The biomass porous carbon, acetylene black and polytetrafluoroethylene obtained in Example 1 were mixed uniformly in a mass ratio of 8:1:1, and N-methylpyrrolidone was used to make a slurry; graphite paper was used as a collective flow, and then the slurry was coated on both surfaces of the graphite paper, and vacuum dried at 60°C and rolled to obtain a thin sheet of supercapacitor electrodes. The obtained two supercapacitor electrodes of the same size were assembled into a supercapacitor, and the electrolyte used was a 5 mol / L KOH aqueous solution.

[0069] Application Example 2-9

[0070] Other conditions are the same as those in Application Example 1, except that the biomass porous carbons are prepared according to Examples 2-9 respectively.

[0071] Comparative Application Example 1-2

[0072] Other conditions are the same as those in Application Example 1, except that the biomass porous carbons are prepared according to Comparative Examples 1-2 respectively.

[0073] Results and Analysis

[0074] The biomass porous carbon prepared in the examples and comparative examples was subjected to the following tests:

[0075] Specific surface area and pore size determination: A Tristar II 3020 fully automatic specific surface and pore size analyzer produced by Micromeritics Instrument Corporation of the United States was used to conduct a low-temperature nitrogen adsorption experiment on the biomass porous carbon prepared in the embodiment and the comparative example to determine the specific surface area and pore size distribution of the porous carbon. The pores with a diameter less than 2nm are micropores; the pores with a diameter in the range of 2 to 50nm are mesopores. The specific data are shown in Table 1.

[0076] Element content determination: The nitrogen, sulfur and oxygen content of the biomass porous carbons prepared in the examples and comparative examples were analyzed using the vario EL cube element analyzer produced by Elementar of Germany. The data are shown in Table 1.

[0077] Table 1 Specific surface area, pore size and element content of biomass porous carbon

[0078]

[0079] It can be seen from Table 1 that compared with the comparative example, the biomass porous carbon prepared by the preparation method of the present invention has a higher specific surface area and a high distribution rate of micropores, with a specific surface area of ​​1800m 2 / g or more, and the microporosity is more than 86%; and the porous carbon contains nitrogen and sulfur elements, with the nitrogen content reaching more than 7% and the sulfur content reaching more than 4%; at the same time, the surface oxygen content of the porous carbon prepared by the present invention is less than 1.5%.

[0080] By comparing Comparative Example 2 with Example 1, it can be seen that although the use of thiourea instead of pyridinethiourea hydrochloride slightly increases the nitrogen content and sulfur content of the porous carbon, its porosity and specific surface area are significantly lower.

[0081] The supercapacitors prepared in the application examples and comparative application examples were subjected to electrochemical performance tests, including specific capacitance curves obtained by scanning at different current densities and cycle stability tests at a current density of 5 A / g. The data are shown in Table 2.

[0082] Table 2 Electrochemical properties of supercapacitors

[0083]

[0084] As can be seen from Table 2, compared with the comparative application examples, the cycle stability and capacitance of the supercapacitors prepared in application examples 1 to 9 are significantly improved, and the capacitance retention rate after 5000 cycles at a current density of 5A / g is as high as 89% or more. At a current density of 1A / g, the specific capacitance is more than 280F / g, at a current density of 10A / g, the specific capacitance is more than 250F / g, and at a high current density of 30A / g, the specific capacitance can still reach more than 180F / g.

[0085] In summary, the biomass porous carbon prepared by the preparation method of the present invention has a strength of 1800m 2 / g or more and a microporosity of more than 86%; and a nitrogen content of more than 7%, a sulfur content of more than 4%, and an oxygen content of less than 1.5%; as an electrode material for supercapacitors, it can significantly improve the cycle stability and capacitance of supercapacitors.

[0086] The above detailed description is a specific description of one feasible embodiment of the present invention. The embodiment is not intended to limit the patent scope of the present invention. Any equivalent implementation or modification that does not deviate from the present invention should be included in the scope of the technical solution of the present invention.

Claims

1. A method for preparing biomass porous carbon for supercapacitors, Its special feature is that The following steps are involved: (S1) Pretreatment: crushing, washing and drying the biomass raw materials in sequence to obtain pretreated biomass; (S2) hydrothermal pre-carbonization: adding the pretreated biomass and pyridinethiourea hydrochloride in a mass ratio of 100:(15-25) to water, heating and heat preservation in a sealed environment, cooling to room temperature after heat preservation, filtering and drying to obtain a solid substance, i.e., hydrothermal carbon; the pyridinethiourea hydrochloride is at least one of 2-pyridinethiourea hydrochloride, 3-pyridinethiourea hydrochloride, 4-pyridinethiourea hydrochloride, and pyridinethione urea; (S3) Pyrolysis carbonization: mixing the hydrothermal carbon and the inorganic base in a mass ratio of 100:(30-50), carbonizing under an inert atmosphere, and then cooling, washing, and drying to obtain pyrolysis carbon; (S4) Deoxidation treatment: placing the pyrolytic carbon in an atmosphere of hydrogen and nitrogen mixed gas at 900-1100°C for reaction, and then cooling and grinding to obtain biomass porous carbon for supercapacitor.

2. The preparation method according to claim 1, It is characterized in that In step (S1), the biomass is at least one of coconut shell, palm shell, walnut shell and apricot shell; the crushing is to crush to 100-400 meshes, and the crushing method adopts air flow crushing, high-speed crushing or ball milling.

3. The preparation method according to claim 1, It is characterized in that The pyridinethiourea hydrochloride is obtained by a preparation method comprising the following steps: dissolving pyridinethiourea in a solvent and adding hydrochloric acid; stirring the solution and heating it under reflux for 4 to 6 hours; filtering after the reaction, washing with water, and drying to obtain pyridinethiourea hydrochloride.

4. The preparation method according to claim 1, It is characterized in that The solid-liquid ratio of the total mass of the pretreated biomass and pyridinethiourea hydrochloride to water in step (S2) is 1g:3~5mL.

5. The preparation method according to claim 1, It is characterized in that The heating and heat preservation treatment in step (S2) is heat preservation at 180-250° C. for 3-5 hours; the drying is drying at 80-120° C. in a blast dryer for 24-48 hours.

6. The preparation method according to claim 1, It is characterized in that In step (S3), the inorganic base is KOH and / or NaOH.

7. The preparation method according to claim 1, It is characterized in that The carbonization conditions of step (S3) are: under an inert atmosphere, heating to 500-700°C at a heating rate of 3-8°C / min, and keeping warm for 2-4 hours; then heating to 800-900°C and keeping warm for 1-3 hours; the inert atmosphere has an oxygen content of less than 1%; the water washing in step (S3) is washing with deionized water until neutral; the drying is drying in an oven at 80-120°C for 24-36 hours.

8. The preparation method according to claim 7, It is characterized in that The inert atmosphere is a nitrogen or argon atmosphere.

9. The preparation method according to claim 1, It is characterized in that In step (S4), the volume fraction of hydrogen in the hydrogen-nitrogen mixed gas is 4%-7%, and the reaction time is 0.5-2h; the grinding is performed by a jet mill, and the particle size D50 after grinding is 6-10μm.