A method for preparing an enhanced high entropy alloy

By forming a coating on the surface of the ball mill beads, the ball milling process is used to uniformly distribute the enhancer in the high-entropy alloy, which solves the problem of uneven content control and dispersion of the enhancer, and improves the performance and yield of the alloy.

CN118421996BActive Publication Date: 2024-11-26GUANGZHOU ZHONGSHAN FASTENER CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410895433.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-11-26
Estimated Expiration
2044-07-05

AI Technical Summary

Technical Problem

The content of reinforcement agents in existing high-entropy alloys is difficult to strictly control, resulting in uneven dispersion of reinforcement agents during mixing, difficult to meet the designed performance requirements, and easy to lose during ball milling, affecting the performance of the alloy.

Method used

By forming a coating on the surface of the ball mill beads, the coating contains metal powder and reinforcement, the coating is used to damage the coating during the ball mill to introduce the reinforcement into the mixture, achieving secondary dispersion and uniform distribution of the reinforcement, ensuring quantitative Enhancement agent content to prevent agglomeration and loss of adhesion.

Benefits of technology

The quantitative and uniform distribution of enhancers is achieved, the strength, corrosion resistance and plasticity of high-entropy alloys are improved, the yield rate of alloy products is improved, and the performance is met.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118421996B_ABST
    Figure CN118421996B_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing an enhanced high entropy alloy, comprising the following steps: according to the formula of the enhanced high entropy alloy to be prepared, multiple metal elements are required and mixed into metal powder, and a required b-mass enhancer is provided; (0.5-10) b-mass of the metal powder and b-mass of the enhancer are applied to the surface of ball milling beads to form a coating to obtain ball milling beads with a coating; the remaining metal powder and the ball milling beads with a coating are placed in a ball mill for ball milling, and the mixture obtained by ball milling is sintered to obtain an enhanced high entropy alloy. This method is applicable to various high entropy alloy systems and various enhancers, and can effectively enhance the strength, corrosion resistance and plasticity of high entropy alloys.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of high entropy alloys, and in particular to a method for preparing an enhanced high entropy alloy. Background Art

[0002] Compared with the single principal element of traditional alloys, high entropy alloys generally have more than five principal elements, and the content of each group of principal elements is similar, ranging from 5% to 35%. High entropy alloys have four unique properties that give them excellent performance, such as hysteresis diffusion effect, crystal nucleus distortion effect and cocktail effect, thus showing excellent wear resistance, high hardness, high strength and other characteristics.

[0003] There are many high entropy alloy systems, which have different excellent properties but also have disadvantages. For example, the AlCoCrFeNi system has the characteristics of high plasticity and low cost, but its hardness is poor. In view of the shortcomings of different alloys, researchers have made targeted improvements to the alloys in different ways, such as introducing reinforcing agents to improve the alloy properties, introducing B elements into high entropy alloys to improve the strength and wear resistance of high entropy alloys, introducing N elements to improve the solid solution properties of high entropy alloys, introducing O elements to improve the plasticity of high entropy alloys, and introducing aluminum oxide to enhance the corrosion resistance of high entropy alloys.

[0004] The content of the reinforcing agent in the high entropy alloy needs to be strictly controlled, because too low a content of the reinforcing agent cannot achieve the expected improvement effect, while too high a content of the reinforcing agent will lead to the degradation of the performance of the high entropy alloy. However, because the amount of the reinforcing agent used is low, generally it accounts for less than 1% or even less than 0.05% by volume of the high entropy alloy. When such a low volume ratio of the reinforcing agent is added to the high entropy alloy for mixing, it is difficult to disperse and it is easy to adhere to the ball milling beads during the ball milling process, causing losses. The content of the reinforcing agent in the high entropy alloy prepared in this way cannot meet the design requirements, and the distribution of the reinforcing agent in the high entropy alloy is uneven, so that a high entropy alloy with satisfactory performance cannot be prepared.

[0005] Therefore, it is necessary to propose a preparation method that can strictly control the content of the reinforcing agent and make the reinforcing agent uniformly distributed in the high entropy alloy. Summary of the invention

[0006] Based on this, it is necessary to provide an enhanced high entropy alloy and a preparation method thereof.

[0007] A method for preparing an enhanced high entropy alloy comprises the following steps:

[0008] According to the formula of the enhanced high entropy alloy to be prepared, multiple metal elements are required and mixed into metal powder, and the required b quality enhancer is also provided;

[0009] Forming a coating on the surface of the ball milling beads by adding (0.5-10) b mass of metal powder and b mass of reinforcing agent to obtain the ball milling beads with coating;

[0010] The remaining metal powder and the coated ball milling beads are placed in a ball mill for ball milling, and the mixture obtained by ball milling is sintered to obtain an enhanced high entropy alloy.

[0011] The preparation method of the enhanced high entropy alloy is to set a coating on the surface of the ball milling bead, wherein the coating contains metal powder and a reinforcing agent prepared according to the formula of the enhanced high entropy alloy, and the reinforcing agent is initially dispersed in the metal powder during the preparation of the coating, and during the ball milling process, the coating material is gradually destroyed and introduced into the ball milled mixture to form a secondary dispersion of the reinforcing agent, thereby preventing the reinforcing agent from agglomerating or adhering to the loss, achieving quantitative and uniform distribution of the reinforcing agent into the finished alloy product, effectively exerting the performance of the reinforcing agent, and improving the yield rate of the alloy product. This method is applicable to various high entropy alloy systems and various reinforcing agents, and can effectively enhance the strength, corrosion resistance and plasticity of the high entropy alloy.

[0012] In one embodiment, the coating is formed by at least one of physical conversion, chemical deposition and adhesion. The physical conversion refers to mixing the raw materials to form a liquid or gaseous state and then forming a coating on the surface of the ball milling beads. The chemical deposition refers to depositing the raw materials containing various elements of the coating on the surface of the ball milling beads and converting them into the desired single substance or compound. The adhesion refers to mixing the raw materials with an adhesive and applying them on the ball milling beads to solidify to form a coating. The above methods can form a uniform coating with suitable adhesion, so that the coating of the ball milling beads can be evenly detached during the ball milling process.

[0013] In one embodiment, the physical conversion method includes: mixing metal powder, reinforcing agent and ball milling beads, and sintering to form a coating. Of course, the coating can also be formed by other conventional physical conversions, such as physical vapor deposition.

[0014] In one embodiment, the chemical deposition method includes: converting the metal powder and the reinforcing agent into a solution or a solid-liquid mixture, precipitating the solution or the solid-liquid mixture on the surface of the ball mill to form a precursor, and then converting the precursor into a coating containing a metal element and a reinforcing agent. Specifically, a sparingly soluble salt or sparingly soluble base containing the total elements contained in the metal powder or the reinforcing agent can be formed, or a precursor containing the total elements can be formed by precipitation of a complexing agent. Specifically, the precursor is converted into a metal oxide by calcination, and then partially or completely converted into a metal element by a reducing agent.

[0015] In one embodiment, the adhesion method includes: mixing metal powder, reinforcing agent and binder, and applying the mixture to the surface of the ball milling beads to form a coating. Specifically, according to the ball milling conditions, an organic binder or an inorganic binder, such as a resin binder or a silicate binder, can be selected.

[0016] In one of the embodiments, the coating is tested during the ball milling process, and when it is determined that the residual rate of the coating is less than 10%, the mixture obtained by ball milling is sintered. Specifically, multiple sampling tests can be performed during the ball milling process. The optional detection method is to weigh the mass of the ball milling beads before coating, after coating and after ball milling, according to the formula: residual rate = (mass after coating - mass after ball milling) / (mass after coating - mass without coating) * 100%. Of course, the residual rate of the coating can also be obtained by physically or chemically stripping the coating, or by thermal gravimetry. Specifically, the ball milling parameters and the preparation method of the coating can be adjusted according to the residual rate of the coating to ensure that the reduced residual rate will not affect the mixing uniformity of the reinforcing phase.

[0017] In one embodiment, (1-2) b mass of metal powder and b mass of reinforcing agent are applied to the surface of the ball mill to form a coating. If the ratio of metal powder is too low, it is difficult to achieve the initial dispersion of the reinforcing agent; if the ratio of metal powder is too high, a thicker coating needs to be prepared when the amount of reinforcing agent added remains unchanged, which makes it difficult to ensure uniform peeling of the coating. The above ratio can achieve uniform mixing of the enhanced type with a low residual rate.

[0018] In one embodiment, the rotation speed of the ball mill is 300-500 r / min, the ball milling time is 20-30 h, and the ball-to-material ratio is (5-10): 1. The ball mill parameters in the above range can ensure that the coating of the ball milling beads is evenly stripped and the residual rate is less than 10%.

[0019] In one embodiment, the reinforcing agent includes at least one element of C, B and O. The reinforcing agent containing the C element is beneficial to improving the toughness of the high entropy alloy, and the B and O elements can improve the mechanical strength of the high entropy alloy. The appropriate reinforcing agent can be selected according to the improvement requirements of the alloy. Specifically, the reinforcing agent includes at least one of graphene, carbon nanotubes and aluminum oxide. Graphene and carbon nanotubes are prone to agglomeration in conventional addition methods, and this solution fixes graphene or carbon nanotubes in the coating in advance, and gradually releases and mixes them into the alloy material during the ball milling process, so as not to cause graphene agglomeration, and can better play the role of graphene in enhancing the plasticity of the material. Aluminum oxide can enhance the corrosion resistance of the material, and can be prepared by forming aluminum hydroxide precipitation on the surface of the ball milling beads and then drying.

[0020] An enhanced high entropy alloy is prepared by the preparation method of the enhanced high entropy alloy.

[0021] The alloy has quantitative and uniformly dispersed reinforcements and has at least one of improved strength, corrosion resistance and plasticity. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 The present invention is a schematic flow chart of a method for preparing an enhanced high entropy alloy according to an embodiment.

[0023] Figure 2 The hardness test results of the high entropy alloys prepared in Examples 1-4, Comparative Example 1 and Comparative Example 2 are shown. DETAILED DESCRIPTION

[0024] For ease of understanding of the application, the application will be described more fully below. The application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the application more thorough and comprehensive.

[0025] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features. In the description of the application, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. In the description of the present application, the meaning of "several" is at least one, such as one, two, etc., unless otherwise clearly and specifically defined.

[0026] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which the present application belongs. The terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.

[0027] In the present application, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.

[0028] In this application, when it comes to numerical ranges, unless otherwise specified, the above numerical ranges are deemed to be continuous and include the minimum and maximum values ​​of the range, as well as each value between such minimum and maximum values. Further, when a range refers to an integer, each integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.

[0029] The percentage contents involved in this application, unless otherwise specified, refer to mass percentage for solid-liquid mixing and solid-solid mixing, and refer to volume percentage for liquid-liquid mixing.

[0030] The percentage concentrations mentioned in this application, unless otherwise specified, refer to the final concentration, which refers to the percentage of the added component in the system after the addition of the component.

[0031] The temperature parameters in this application, unless otherwise specified, allow for both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows the temperature to fluctuate within the accuracy range of instrument control.

[0032] The "particles" mentioned in this application, or materials with a defined particle size distribution, are not necessarily spherical in shape, but may be irregular, primary particles or secondary particles. The particle size of irregular particles is the average of their maximum diameter and minimum diameter.

[0033] Example 1: A method for preparing an enhanced alloy, wherein the enhanced alloy is AlFeMnCoCrB 0.05 , various raw materials were weighed according to the requirements of preparing 56 kg of enhanced alloy, the mass of the metal powder obtained by mixing the five elements of Al, Fe, Mn, Co and Cr was 56 kg, and the mass of the reinforcing agent B (boron) was 125 g; 1250 g of metal powder, 125 g of reinforcing agent B and 40 g of PVA binder were mixed and coated on ball milling beads (zirconia ball milling beads with a diameter of 10 mm, the same below) to form a coating; the remaining metal powder was placed in a ball mill, the ball milling beads with the coating were placed in the ball mill, the ball mill was started, the ball mill speed was 500 r / min, the ball milling time was 20 h, the ball-to-material ratio was 5:1, and the residual rate of the ball milling bead coating after ball milling was detected to be 1.02% (calculation formula: residual rate = (mass after coating - mass after ball milling) / (mass after coating - mass without coating) * 100%), and the upper, middle and bottom parts of the ball milling jar were sampled and analyzed after ball milling to obtain the distribution of each component in the high entropy alloy.

[0034] The ball-milled mixture was transferred to a vacuum induction melting furnace and repeatedly melted 5 times in an argon atmosphere at a sintering temperature of 1000 degrees Celsius. The obtained alloy mother ingot was cast in a copper mold and kept at 1000 degrees Celsius for 3 hours to obtain an alloy ingot.

[0035] Example 2: A method for preparing an enhanced alloy, wherein the enhanced alloy is AlFeMnCoCrB 0.05, various raw materials were weighed according to the requirements of preparing 56 kg of enhanced alloy, the mass of the metal powder obtained by mixing the five elements of Al, Fe, Mn, Co, and Cr was 56 kg, and the mass of the enhancer B was 125 g; 62.5 g of metal powder, 125 g of enhancer B and 6 g of PVA binder were mixed and coated on the ball milling beads for curing to form a coating; the remaining metal powder was placed in a ball mill, the ball milling beads with the coating were placed in the ball mill, the ball mill was started, the ball mill speed was 500 r / min, the ball milling time was 20 h, the ball-to-material ratio was 5:1, and the residual rate of the ball milling bead coating after ball milling was detected to be 2.68% (calculation formula: residual rate = (mass after coating - mass after ball milling) / (mass after coating - mass without coating) * 100%), and the upper, middle and bottom parts of the ball milling jar were sampled and analyzed after ball milling to obtain the distribution of each component in the high entropy alloy.

[0036] The ball-milled mixture was transferred to a vacuum induction melting furnace and repeatedly melted 5 times in an argon atmosphere at a sintering temperature of 1000 degrees Celsius. The obtained alloy mother ingot was cast in a copper mold and kept at 1000 degrees Celsius for 3 hours to obtain an alloy ingot.

[0037] Example 3: A method for preparing an enhanced alloy, wherein the enhanced alloy is AlFeMnCoCrB 0.05 , various raw materials were weighed according to the requirements of preparing 56kg enhanced alloy, the mass of the metal powder obtained by mixing the five elements of Al, Fe, Mn, Co and Cr was 56kg, and the mass of the enhancer B was 125g; 250g of metal powder, 125g of enhancer B and 20g of PVA binder were mixed and coated on the ball milling beads for curing to form a coating; the remaining metal powder was placed in a ball mill, the ball milling beads with the coating were placed in the ball mill, the ball mill was started, the ball mill speed was 500r / min, the ball milling time was 20h, the ball-to-material ratio was 5:1, and the residual rate of the ball milling bead coating after ball milling was detected to be 1.23% (calculation formula: residual rate = (mass after coating - mass after ball milling) / (mass after coating - mass without coating) * 100%), and the upper, middle and bottom parts of the ball milling jar were sampled and analyzed after ball milling to obtain the distribution of each component in the high entropy alloy.

[0038] The ball-milled mixture was transferred to a vacuum induction melting furnace and repeatedly melted 5 times in an argon atmosphere at a sintering temperature of 1000 degrees Celsius. The obtained alloy mother ingot was cast in a copper mold and kept at 1000 degrees Celsius for 3 hours to obtain an alloy ingot.

[0039] Example 4: A method for preparing an enhanced alloy, wherein the enhanced alloy is AlFeMnCoCrB 0.01, various raw materials were weighed according to the requirements of preparing 56 kg of enhanced alloy, the mass of the metal powder obtained by mixing the five elements of Al, Fe, Mn, Co and Cr was 56 kg, and the mass of the enhancer B was 25 g; 125 g of metal powder, 25 g of enhancer B and 4 g of PVA binder were mixed and coated on the ball milling beads for curing to form a coating; the remaining metal powder was placed in a ball mill, the ball milling beads with the coating were placed in the ball mill, the ball mill was started, the ball mill speed was 300 r / min, the ball milling time was 20 h, the ball-to-material ratio was 10:1, and the residual rate of the ball milling bead coating after ball milling was detected to be 2.35% (calculation formula: residual rate = (mass after coating - mass after ball milling) / (mass after coating - mass not coated) * 100%), and the upper, middle and bottom parts of the ball milling jar were sampled and analyzed after ball milling to obtain the distribution of each component in the high entropy alloy.

[0040] The ball-milled mixture was transferred to a vacuum induction melting furnace and repeatedly melted 5 times in an argon atmosphere at a sintering temperature of 1000 degrees Celsius. The obtained alloy mother ingot was cast in a copper mold and kept at 1000 degrees Celsius for 3 hours to obtain an alloy ingot.

[0041] Example 5: A method for preparing a reinforced alloy, wherein the reinforced alloy is carbon nanotubes (mass fraction 0.2%) / AlFeMnCoCr. Various raw materials are weighed according to the requirement for preparing 56 kg of the reinforced alloy. The mass of the metal powder obtained by mixing the five elements of Al, Fe, Mn, Co and Cr is 56 kg. 1250 g of the metal powder, 112 g of the reinforcing carbon nanotubes and ball milling beads are placed in a ball mill at 300 r / min for 12 h, and then transferred to an inert gas atmosphere and fully sintered at 1000°C for 10 h to obtain coated ball milling beads; the remaining metal powder is placed in a ball mill, the coated ball milling beads are placed in the ball mill, the ball mill is started, the ball mill speed is 500r / min, the ball milling time is 20h, the ball-to-material ratio is 5:1, and the residual rate of the ball milling bead coating after ball milling is detected to be 8.23% (calculation formula: residual rate = (mass after coating - mass after ball milling) / (mass after coating - mass without coating) * 100%). After ball milling, the upper, middle and bottom parts of the ball mill jar are sampled and analyzed to obtain the distribution of each component in the high entropy alloy.

[0042] The ball-milled mixture was transferred to a vacuum induction melting furnace and repeatedly melted 5 times in an argon atmosphere at a sintering temperature of 1000 degrees Celsius. The obtained alloy mother ingot was cast in a copper mold and kept at 1000 degrees Celsius for 3 hours to obtain an alloy ingot.

[0043] Example 6: A method for preparing an enhanced alloy, wherein the enhanced alloy is AlFeMnCoCrO 0.05, various raw materials were weighed according to the requirements for preparing 56 kg of enhanced alloy, and the mass of metal powder obtained by mixing five elements of Al, Fe, Mn, Co, and Cr was 56 kg; 1.87 kg of the mixture was dissolved in dilute sulfuric acid, and after the reaction was complete, ball milling beads were added, and then an excess of 1 mol / L sodium hydroxide and 10 g / L of complexing agent were added to form a precipitation layer on the surface of the ball milling beads, and the ball milling beads were calcined at 1000°C for 10 hours to obtain coated ball milling beads; the remaining metal The powder is placed in a ball mill, and the coated ball milling beads are placed in the ball mill. The ball mill is started, the ball mill speed is 500r / min, the ball milling time is 20h, the ball-to-material ratio is 5:1, and the residual rate of the ball milling bead coating after ball milling is 7.24% (calculation formula: residual rate = (mass after coating - mass after ball milling) / (mass after coating - mass without coating) * 100%). After ball milling, the upper, middle and bottom parts of the ball mill jar are sampled and analyzed to obtain the distribution of each component in the high entropy alloy.

[0044] The ball-milled mixture was transferred to a vacuum induction melting furnace and repeatedly melted 5 times in an argon atmosphere at a sintering temperature of 1000 degrees Celsius. The obtained alloy mother ingot was cast in a copper mold and kept at 1000 degrees Celsius for 3 hours to obtain an alloy ingot.

[0045] Comparative Example 1: A method for preparing an enhanced alloy, wherein the enhanced alloy is AlFeMnCoCrB 0.05 , various raw materials were weighed according to the demand for preparing 56 kg of enhanced alloy, the mass of the metal powder obtained by mixing the five elements of Al, Fe, Mn, Co, and Cr was 56 kg, and the mass of the enhancer B was 125 g; the metal powder and 125 g of the enhancer B were placed in a ball mill, the uncoated ball milling beads were placed in the ball mill, the ball mill was started, the ball mill speed was 500 r / min, the ball milling time was 20 h, the ball-to-material ratio was 5:1, and after ball milling, the upper, middle and bottom of the ball mill jar were sampled and analyzed to obtain the distribution of each component in the high entropy alloy powder.

[0046] The ball-milled mixture was transferred to a vacuum induction melting furnace and repeatedly melted 5 times in an argon atmosphere at a sintering temperature of 1000 degrees Celsius. The obtained alloy mother ingot was cast in a copper mold and kept at 1000 degrees Celsius for 3 hours to obtain an alloy ingot.

[0047] Comparative Example 2: A method for preparing an enhanced alloy, wherein the enhanced alloy is AlFeMnCoCrB 0.05, various raw materials were weighed according to the requirements of preparing 56 kg of enhanced alloy, the mass of the metal powder obtained by mixing the five elements of Al, Fe, Mn, Co and Cr was 56 kg, and the mass of the enhancer B was 125 g; 125 g of the enhancer B was mixed with 4 g of PVA binder and then coated on the ball milling beads for curing to form a coating; the metal powder was placed in a ball mill, the ball milling beads with the coating were placed in the ball mill, the ball mill was started, the ball mill speed was 500 r / min, the ball milling time was 20 h, the ball-to-material ratio was 5:1, and the residual rate of the ball milling bead coating after ball milling was detected to be 3.07% (calculation formula: residual rate = (mass after coating - mass after ball milling) / (mass after coating - mass without coating) * 100%), and the upper, middle and bottom parts of the ball milling jar were sampled and analyzed after ball milling to obtain the distribution of each component in the high entropy alloy.

[0048] The ball-milled mixture was transferred to a vacuum induction melting furnace and repeatedly melted 5 times in an argon atmosphere at a sintering temperature of 1000 degrees Celsius. The obtained alloy mother ingot was cast in a copper mold and kept at 1000 degrees Celsius for 3 hours to obtain an alloy ingot.

[0049] Hardness test method: Test according to the national standard GB / T 7997-2014 "Vickers hardness test method for cemented carbide" and draw according to the test results Figure 2 .

[0050] Table 1 Distribution of components (mass %) in the high entropy alloy powders of Examples 1-6 and Comparative Examples 1-2.

[0051] According to Table 1 and Figure 2 From the data, it can be seen that although the dispersion effect of B in Comparative Example 2 is improved compared with Comparative Example 1, it is still not as good as Example 1. This is because it lacks the initial dispersion of the metal powder on the reinforcing agent during the coating preparation process, and the reinforcing agent is easy to agglomerate on the surface of the ball milling beads during the ball milling process. The content of B powder in the bottom of Comparative Example 1-2 is too low and the distribution in the upper part is too high, which leads to the inability of the reinforcing agent to perform normally. Figure 2 The results show that a slight change in the B content can have a significant effect on the hardness of the alloy, and the reinforcing agent content distribution of Examples 1-4 is more uniform and has low loss, which can ensure that the reinforcing agent content in the high entropy alloy powder is within the design value. Figure 2From the data, it can be seen that Examples 1-4 not only have higher hardness, but also have smaller deviations, which indicates that the distribution of B is more uniform. This is because the preparation method of the enhanced high entropy alloy of Examples 1-4, by setting a coating on the surface of the ball milling beads, the coating contains metal powder and a reinforcing agent prepared according to the formula of the enhanced high entropy alloy, and the reinforcing agent is initially dispersed in the metal powder during the preparation of the coating, and during the ball milling process, the coating material is gradually destroyed and introduced into the ball milled mixture to form a secondary dispersion of the reinforcing agent, thereby preventing the reinforcing agent from agglomerating or adhering to the loss, achieving quantitative and uniform distribution of the reinforcing agent to the finished alloy product, effectively exerting the performance of the reinforcing agent, and improving the yield rate of the alloy product. The hardness of Example 3 is higher than that of Example 2, and the deviation is smaller, because the preferred ratio of reinforcing agent / metal powder is used in the preparation process of the coating, which achieves better initial dispersion.

[0052] According to the coating residual rate of each embodiment and the data in Table 1, it can be seen that the coating residual rate of embodiments 1-4 is significantly lower than that of embodiments 5-6. This is because embodiments 5-6 all need to form the coating by sintering, and the coating strength is too high, which is not conducive to peeling during the ball milling process, thus resulting in the amount of reinforcing agent added being lower than the designed value. Embodiments 1-4 form the coating by adhesion with suitable strength, which can be fully and evenly peeled off, and can achieve more quantitative addition of reinforcing agent.

[0053] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0054] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing an enhanced high entropy alloy, characterized in that: The steps include: The enhanced high entropy alloy is AlFeMnCoCrB 0.05 , according to the formula of the enhanced high entropy alloy to be prepared, multiple metal elements are prepared and mixed into metal powders, and the required b quality enhancer is prepared; Forming a coating on the surface of a ball milling bead with (0.5-10) b mass of the metal powder and b mass of the reinforcing agent to obtain the ball milling bead with the coating, wherein the reinforcing agent includes B; The remaining metal powder and the ball milling beads with the coating are placed in a ball mill for ball milling, and the mixture obtained by ball milling is sintered to obtain the enhanced high entropy alloy; the coating is formed by adhesion; the coating is tested during the ball milling process, and when it is determined that the residual rate of the coating is less than 10%, the mixture obtained by ball milling is sintered.

2. The method for preparing an enhanced high entropy alloy according to claim 1, characterized in that: The adhesion method includes: mixing the metal powder, the reinforcing agent and the binder, and applying the mixture on the surface of the ball milling beads to form the coating.

3. The method for preparing an enhanced high entropy alloy according to claim 1, characterized in that: The metal powder (1-2) b mass and the reinforcing agent (b mass) are placed on the surface of the ball milling beads to form the coating.

4. The method for preparing an enhanced high entropy alloy according to claim 1, characterized in that: The rotation speed of the ball mill is 300-500 r / min, the ball milling time is 20-30 h, and the ball-to-material ratio is (5-10):1.