A CeO2 / Ti3C2T x Composite material and preparation method and application thereof
The spherical CeO2/few-layer Ti3C2Tx composite material was prepared by hydrothermal method and surface charge control strategy, which solved the problem of poor gas sensing performance of a single MXene material, achieved efficient detection of formaldehyde gas with good repeatability, and expanded the scope of application.
Patent Information
- Application Number
- CN202410512104.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-26
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-04-26
AI Technical Summary
Sensors based on a single MXene material have poor gas-sensing performance and narrow application range, and are limited by the carrier conduction mechanism, narrow band gap and low chemical stability of pure oxides.
The hydrothermal method and surface charge control strategy were used to prepare spherical CeO2/few-layer Ti3C2Tx composite materials. Few-layer Ti3C2Tx nanosheets were prepared through ultrasonic extraction and the surface charge of CeO2 was controlled to form spherical CeO2/few-layer Ti3C2Tx composite materials, which enhanced carrier transmission and reaction rate.
It significantly improves the gas-sensing reaction rate and the specific surface area of the material, achieving efficient detection of formaldehyde gas. It combines the performance advantages of CeO2 and Ti3C2Tx materials, is suitable for mass preparation and has good repeatability.
Smart Images

Figure CN118425246B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of gas-sensitive material preparation, and in particular to a CeO2 / Ti3C2T x Composite material and preparation method and application thereof. Background Art
[0002] Ce is the most abundant rare earth element on earth. Its oxide CeO2 has a fluorite structure and has many oxygen vacancies, dangling bonds and lattice defects on its surface, which help to absorb oxygen on its surface and convert it into oxygen anions, making it suitable for gas-sensitive materials. 3+ / Ce 4+ The reversible transformation characteristics between ions make CeO2 occupy an important position in the field of catalysis.
[0003] MXene materials have a two-dimensional layered structure, high electrical conductivity, and high signal-to-noise ratio. They can be obtained by selectively etching the A atomic layer corresponding to the three-dimensional bulk MAX phase and then ultrasonically dispersing it. The most widely used MXene material is Ti3C2T x This type of material also has similar physical and chemical properties as graphene, such as conductivity and hydrophilicity, and surface terminals that are easily regulated, showing unique application prospects in many fields such as energy storage, catalysis, and sensing.
[0004] However, due to the special carrier conduction mechanism of pure oxides, the narrow band gap and low chemical stability of MXene materials, the gas sensing performance of sensors based on a single material is poor and the application range is narrow. Summary of the invention
[0005] The purpose of the present invention is to overcome the defects of the prior art and propose a CeO2 / Ti3C2T x Composite materials, preparation methods and applications thereof, a spherical CeO2 / few-layer Ti3C2T composite material was prepared by hydrothermal method and surface charge control strategy x Composite materials can combine the performance advantages of both materials and are suitable for large-scale preparation, while also achieving efficient detection of formaldehyde gas.
[0006] To achieve the above object, the present invention adopts the following specific technical solutions:
[0007] CeO2 / Ti3C2T provided by the present invention x The method for preparing the composite material comprises the following steps:
[0008] S1. Disperse cerium nitrate in deionized water and add ethylene glycol to obtain a mixed solution, add the mixed solution into a reactor, heat and keep it warm, wash it, and then centrifuge it to obtain a precipitate, dry the precipitate, and then anneal it to obtain spherical CeO2;
[0009] S2. Disperse LiF in deionized water in a water bath, add concentrated hydrochloric acid and Ti3AlC2 in sequence, stir and wash, collect the slurry solution, treat it ultrasonically in an ice-water mixture, centrifuge to obtain the supernatant and freeze-dry to obtain Ti3C2T x Nanosheets;
[0010] S3, spherical CeO2 was dispersed in ethanol, hexadecyltrimethylammonium bromide (CTAB) was added, stirred and centrifuged to dry; the dried powder was dispersed in deionized water in a water bath, and Ti3C2T x The nanosheets were stirred and placed in a reactor for heating and heat preservation to react. The solution after the reaction was washed, the precipitate was collected by centrifugation and dried to obtain CeO2 / Ti3C2T x Composite materials.
[0011] Furthermore, in step S1, the stirring time is 30 to 50 minutes, the reactor temperature is 120 to 140° C., and the insulation time is 24 to 36 hours.
[0012] Furthermore, in step S1, the dried precipitate is annealed in a muffle furnace, the annealing temperature is 500-550° C., and the annealing holding time is 1-2 hours.
[0013] Furthermore, in step S2, the water bath environment temperature is 40-50°C, the stirring time is 36-48 hours, the slurry solution is collected when the pH value of the supernatant is 6-7 after washing, the ultrasonic treatment time is 1-3 hours, and the freeze-drying time is 36-48 hours.
[0014] Further, in step S3, after adding CTAB, the stirring time is 2 to 4 hours, the water bath environment temperature is 40 to 60°C, and Ti3C2T x The stirring time of the nanosheets is 6 to 8 hours, the reactor temperature is 110 to 120° C., and the insulation time is 5 to 8 hours.
[0015] A CeO2 / Ti3C2T x The composite material is prepared by the above preparation method.
[0016] CeO2 / Ti3C2T prepared by the above preparation method x Application of composite materials in formaldehyde gas detection.
[0017] The present invention can achieve the following technical effects:
[0018] The preparation method provided by the present invention is to prepare a few-layer Ti3C2T by ultrasonic extraction in an ice bath environment. xNanosheet materials, few-layer structures effectively avoid material agglomeration, thereby improving the interaction efficiency between charges. Spherical CeO2 / few-layer Ti3C2T3C2 / Ti ... x Composite materials. In the gas sensing reaction process, CeO2 3+ With Ce 4+ The ions can be exchanged reversibly and quickly, which significantly improves the reaction rate. The high conductivity of MXene is also conducive to the transport of carriers, which can also speed up the reaction. The special spherical and few-layer flake structures increase the specific surface area of the two basic materials, which helps to adsorb more oxygen anions to participate in the reaction. The prepared composite material can have both spherical CeO2 and few-layer Ti3C2T x The performance advantages of the two materials of the nanosheet make it suitable for large-scale preparation. In addition, the composite material can also achieve efficient detection of formaldehyde gas. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is a schematic diagram of a preparation method according to an embodiment of the present invention.
[0020] Figure 2 It is a SEM spectrum of the CeO2 sample provided according to the embodiment of the present invention.
[0021] Figure 3 It is Ti3C2T provided by the embodiment of the present invention. x SEM images of the samples.
[0022] Figure 4 CeO2 / Ti3C2T provided according to an embodiment of the present invention x SEM images of the composite samples.
[0023] Figure 5 It is Ti3C2T provided by the embodiment of the present invention. x 、CeO2 / Ti3C2T x , XRD patterns of CeO2 samples.
[0024] Figure 6 It is Ti3C2T provided by the embodiment of the present invention. x 、CeO2 / Ti3C2T x , Raman spectra of CeO2 samples.
[0025] Figure 7 CeO2 / Ti3C2T provided according to an embodiment of the present invention x , dynamic response / recovery curve of CeO2 sample to 300ppm formaldehyde gas at 270℃.
[0026] Figure 8 CeO2 / Ti3C2T provided according to an embodiment of the present invention x Response curve of composite materials to different concentrations of formaldehyde gas.
[0027] Fig. 9 CeO2 / Ti3C2T provided according to an embodiment of the present invention x Repeatability response test curve of composite materials to formaldehyde gas. DETAILED DESCRIPTION
[0028] Hereinafter, embodiments of the present invention will be described with reference to the accompanying drawings. In the following description, the same modules are represented by the same reference numerals. In the case of the same reference numerals, their names and functions are also the same. Therefore, the detailed description thereof will not be repeated.
[0029] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and do not constitute a limitation of the present invention.
[0030] The present invention provides a CeO2 / Ti3C2T x A method for preparing a composite material, wherein the process of the preparation method is as follows Figure 1 As shown, the following steps are included:
[0031] S1. Disperse cerium nitrate in deionized water and add ethylene glycol to obtain a mixed solution, add the mixed solution into a reactor, heat and keep warm, wash, and then centrifuge to obtain a precipitate, dry the precipitate, and then anneal to obtain spherical CeO2.
[0032] S2. Disperse LiF in deionized water in a water bath, add concentrated hydrochloric acid and Ti3AlC2 in sequence, stir and wash, collect the slurry solution, treat it ultrasonically in an ice-water mixture, centrifuge to obtain the supernatant and freeze-dry to obtain Ti3C2T x Nanosheets.
[0033] S3, spherical CeO2 was dispersed in ethanol, hexadecyltrimethylammonium bromide (CTAB) was added, stirred and centrifuged to dry; the dried powder was dispersed in deionized water in a water bath, and Ti3C2T x The nanosheets were stirred and placed in a reactor for heating and heat preservation to react. The solution after the reaction was washed, the precipitate was collected by centrifugation and dried to obtain CeO2 / Ti3C2T x Composite materials.
[0034] In step S1, the stirring time is 30 to 50 minutes, the reactor temperature is 120 to 140° C., and the heat preservation time is 24 to 36 hours. The dried precipitate is annealed in a muffle furnace at a temperature of 500 to 550° C. and a heat preservation time of 1 to 2 hours.
[0035] In step S2, the water bath environment temperature is 40-50°C, the stirring time is 36-48 hours, the slurry solution is collected when the pH value of the supernatant is 6-7 after washing, the ultrasonic treatment time is 1-3 hours, and the freeze-drying time is 36-48 hours.
[0036] In step S3, after adding CTAB, the stirring time is 2 to 4 hours, the water bath environment temperature is 40 to 60°C, and Ti3C2T x The stirring time of the nanosheets is 6 to 8 hours, the reactor temperature is 110 to 120° C., and the insulation time is 5 to 8 hours.
[0037] The preparation method provided by the present invention is described below in conjunction with specific examples.
[0038] Example 1
[0039] Disperse 1.302g of cerium nitrate in 5mL of deionized water, slowly drip 30mL of ethylene glycol, and continue stirring for 30min. Pour the mixed solution into a 100mL reactor, with a target temperature of 140℃ and a holding time of 24h. The solution obtained after the reaction was cross-cleaned twice with water and anhydrous ethanol, and the precipitate was collected by centrifugation and dried at 70℃. The dried powder sample was annealed in a muffle furnace, with a target temperature of 500℃ and a holding time of 1 hour to obtain spherical CeO2 with a diameter distribution in the range of 200 to 500nm. The scanning electron microscope image (SEM) results are as follows: Figure 2 shown.
[0040] In a 40°C water bath, 1.6 g LiF was dispersed in 25 mL deionized water, 15 mL of 12 mol / L concentrated hydrochloric acid was slowly added, and 1 g Ti3AlC2 powder sample was slowly added to the above solution in 10 times, and stirred for 48 hours to complete the etching. Washed with deionized water several times until the pH value of the supernatant was 6.5. The black slurry solution was collected and ultrasonicated for 1 hour in an ice-water mixing environment, and the supernatant was collected by centrifugation. After freeze-drying for 48 hours, a few-layer Ti3C2T x Nanosheets, scanning electron microscope images are shown in Figure 3 shown.
[0041] Take 50 mg of spherical CeO2 and disperse it in 20 mL of ethanol, add 4 mg of hexadecyltrimethylammonium bromide (CTAB), stir for 3 hours, and then centrifuge and dry. Take 30 mg of CeO2 powder sample treated with CTAB, disperse it in 20 mL of deionized water, place it in a 40°C water bath, and slowly add 2 mg of few-layer Ti3C2T x After continuous stirring for 6 hours, the mixed solution was poured into a 100 mL reactor, the target temperature was 120 °C, and the heat preservation time was 6 hours. The reacted solution was repeatedly washed with deionized water and anhydrous ethanol, the precipitate was collected by centrifugation, and dried at 70 °C to obtain spherical CeO2 / few-layer Ti3C2T x Composite materials, SEM images are shown in Figure 4 shown.
[0042] Example 2
[0043] Disperse 1.302g of cerium nitrate in 5mL of deionized water, slowly drip 30mL of ethylene glycol, continue stirring for 30min, pour the mixed solution into a 100mL reactor, target temperature 120℃, keep warm for 24h. The solution obtained after the reaction was cross-washed twice with water and anhydrous ethanol, centrifuged to collect the precipitate, and dried at 70℃. Anneal the dried powder sample in a muffle furnace, target temperature 500℃, keep warm for 1 hour, and obtain spherical CeO2.
[0044] In a 40°C water bath, 1.6 g LiF was dispersed in 25 mL deionized water, 15 mL of 12 mol / L concentrated hydrochloric acid was slowly added, and 1 g Ti3AlC2 powder sample was slowly added to the above solution in 10 times, and stirred for 36 hours to complete the etching. Washed with deionized water several times until the pH value of the supernatant was 6. The black slurry solution was collected and ultrasonicated for 1 hour in an ice-water mixing environment, and the supernatant was collected by centrifugation. After freeze-drying for 36 hours, a few-layer Ti3C2T x Nanosheets.
[0045] Take 50 mg of spherical CeO2 and disperse it in 20 mL of ethanol, add 4 mg of hexadecyltrimethylammonium bromide (CTAB), stir for 2 hours, and then centrifuge and dry. Take 30 mg of CeO2 powder sample treated with CTAB, disperse it in 20 mL of deionized water, place it in a 40°C water bath, and slowly add 2 mg of few-layer Ti3C2T x After continuous stirring for 6 h, the mixed solution was poured into a 100 mL reactor, the target temperature was 110 °C, and the heat preservation time was 5 h. The reacted solution was repeatedly washed with deionized water and anhydrous ethanol, the precipitate was collected by centrifugation, and dried at 70 °C to obtain spherical CeO2 / few-layer Ti3C2T x Composite materials.
[0046] Example 3
[0047] Disperse 1.302g of cerium nitrate in 5mL of deionized water, slowly drip 30mL of ethylene glycol, continue stirring for 50min, pour the mixed solution into a 100mL reactor, target temperature 140℃, keep warm for 36h. The solution obtained after the reaction was cross-washed twice with water and anhydrous ethanol, centrifuged to collect the precipitate, and dried at 70℃. Anneal the dried powder sample in a muffle furnace, target temperature 550℃, keep warm for 2 hours, and obtain spherical CeO2.
[0048] In a 50°C water bath, 1.6 g LiF was dispersed in 25 mL deionized water, 15 mL of 12 mol / L concentrated hydrochloric acid was slowly added, and 1 g Ti3AlC2 powder sample was slowly added to the above solution in 10 times, and stirred for 48 hours to complete the etching. Washed with deionized water several times until the pH value of the supernatant was 7. The black slurry solution was collected and ultrasonicated for 3 hours in an ice-water mixing environment, and the supernatant was collected by centrifugation. After freeze-drying for 48 hours, a few-layer Ti3C2T x Nanosheets.
[0049] Take 50 mg of spherical CeO2 and disperse it in 20 mL of ethanol, add 4 mg of hexadecyltrimethylammonium bromide (CTAB), stir for 4 hours, and then centrifuge and dry. Take 30 mg of CeO2 powder sample treated with CTAB, disperse it in 20 mL of deionized water, place it in a water bath at 60 ° C, and slowly add 2 mg of few-layer Ti3C2T x After continuous stirring for 8 h, the mixed solution was poured into a 100 mL reactor, the target temperature was 120 °C, and the heat preservation time was 8 h. The reacted solution was repeatedly washed with deionized water and anhydrous ethanol, the precipitate was collected by centrifugation, and dried at 70 °C to obtain spherical CeO2 / few-layer Ti3C2T x Composite materials.
[0050] Next, the CeO2, Ti3C2T prepared in Example 1 x Samples and CeO2 / Ti3C2T x The composite material was tested to verify the preparation method provided by the present invention and the effect of the prepared composite material.
[0051] The Ti3C2T prepared in Example 1 x 、CeO2 / Ti3C2T x The X-ray diffraction (XRD) test was carried out on three samples of CeO2. The XRD spectrum results are shown in Figure 5After comparing with the standard card in the crystallographic database, it can be determined that the spherical CeO2 is in good agreement with the standard card (PDF#81-0792). The curve (a) at 8.03° represents Ti3C2T x The (002) characteristic peak of the phase represents CeO2 / Ti3C2T x In the (b) curve of the composite material, the diffraction peak belonging to CeO2 can also be observed, and no diffraction peaks of other impurities appear.
[0052] Ti3C2T x 、CeO2 / Ti3C2T x 、The Raman spectrum of CeO2 samples is as follows Figure 6 As shown, (a) 200cm -1 A representing Ti atom appears near the position 1g The vibration peak outside the symmetric plane is 460 cm in the curve (c). -1 F, which represents the Ce-O symmetric vibration, appears near the position 2g The curve (b) representing the composite material shows characteristic peaks of the two materials. After comparison, it is found that the peak position has shifted, proving that CeO2, Ti3C2T x The two materials were able to be combined successfully.
[0053] The prepared CeO2 / Ti3C2T x The dynamic response and recovery tests of CeO2 samples were carried out. The dynamic response / recovery curve results are shown in Figure 7 Pure CeO2 has almost no response to formaldehyde gas. Under the same conditions, CeO2 / Ti3C2T x The composite material responds significantly to 300ppm formaldehyde gas, with response and recovery times of 4s and 1s respectively. Faster response and recovery rates are conducive to timely response and more ideal application effects.
[0054] CeO2 / Ti3C2T x The response curve of the composite material to different concentrations of formaldehyde gas is shown in Figure 8 As shown, within the concentration range of 100 to 500 ppm, it can be seen that the response value increases with the increase of gas concentration, and the recovery state is good.
[0055] CeO2 / Ti3C2T x The repeatability test results of composite materials for formaldehyde gas are as follows: Fig. 9 As shown in the figure, in the 8-cycle test, the composite material showed good repeatability, and the response state of each cycle maintained good consistency. The gas sensing test results show that spherical CeO2 / few-layer Ti3C2T xThe composite material can not only respond quickly to formaldehyde gas and recover in time, but also has good repeatability, making it an ideal formaldehyde gas detection material.
[0056] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0057] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
[0058] The above specific implementations of the present invention do not constitute a limitation on the protection scope of the present invention. Any other corresponding changes and modifications made based on the technical concept of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A CeO2 / Ti3C2T x The application of composite materials in formaldehyde gas detection is characterized in that: The CeO2 / Ti3C2T x The preparation of the composite material includes the following steps: S1. Disperse cerium nitrate in deionized water and add ethylene glycol, stir for 30-50 min to obtain a mixed solution, add the mixed solution into a reactor at 120-140° C. and heat for 24-36 h, then wash, centrifuge to obtain a precipitate, dry the precipitate, and anneal it in a muffle furnace to obtain spherical CeO2, the annealing temperature is 500-550° C., and the annealing insulation time is 1-2 h; S2. Disperse LiF in deionized water at 40-50°C in a water bath, add concentrated hydrochloric acid and Ti3AlC2 in sequence, stir for 36-48h and then wash until the pH value of the supernatant is 6-7. Collect the slurry solution and treat it ultrasonically for 1-3h in an ice-water mixture, centrifuge to obtain the supernatant and freeze-dry for 36-48h to obtain Ti3C2T x Nanosheets; S3, spherical CeO2 was dispersed in ethanol, hexadecyltrimethylammonium bromide was added, stirred for 2-4 hours and then centrifuged and dried; the dried powder was dispersed in deionized water in a water bath at 40-60℃, and Ti3C2T x The nanosheets were stirred for 6 to 8 hours and then placed in a reactor at 110 to 120°C for 5 to 8 hours for reaction. The solution after the reaction was washed, the precipitate was collected by centrifugation and dried to obtain CeO2 / Ti3C2T x Composite materials.
Citation Information
Cited By
Straw confinement self-assembly cobalt-oxygen-based three-dimensional composite material as well as preparation method and application thereof
CN122627475A