Composite diaphragm, cerium oxide with oxygen vacancies, preparation method and application thereof
By using high oxygen vacancy cerium oxide (CeO2-x) material on the lithium-ion battery separator, the problems of poor constant current charging performance and thermal runaway of lithium batteries at high rates are solved, achieving higher battery safety and cycle performance, simple process, low cost, and suitable for large-scale applications.
Patent Information
- Application Number
- CN202410898964.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-05
AI Technical Summary
Existing lithium-ion battery separators have poor constant-current charging performance at high rates, and conventional ceramic coatings cannot effectively prevent thermal runaway, resulting in battery heat accumulation and the generation of chemically reactive oxygen species, affecting battery safety and cycle performance.
A cerium oxide (CeO2-x) material is used, whose surface has a high proportion of (111) crystal planes and oxygen vacancies. By adding a reducing agent to an acidic solution for deoxidation treatment, a material with high oxygen vacancy concentration and stability is prepared. A large proportion of (111)-CeO2-x is used as a functional coating for separators to enhance the thermal stability and ion migration capabilities of lithium batteries.
It effectively delays the degree of thermal runaway of lithium batteries, improves the migration ability of lithium ions at the electrode electrolyte interface, enhances the safety and cycle performance of the battery, and has a simple process and low cost, making it suitable for large-scale applications.
Smart Images

Figure CN118431673B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of lithium batteries, and in particular to a composite diaphragm, cerium oxide, and a preparation method and application thereof. Background Art
[0002] As one of the key components of lithium-ion batteries, the diaphragm not only determines the capacity and cycle performance of lithium-ion batteries, but also plays a vital role in safety performance. The performance of the diaphragm directly affects the overall performance of the lithium-ion battery.
[0003] At present, the industry generally adopts the method of coating a layer of ceramic coating (such as aluminum oxide) on the surface of the diaphragm. On the one hand, it improves the high-temperature dimensional stability of the diaphragm, consumes impurities in the electrolyte and increases the cycle life; on the other hand, it improves the wettability and liquid absorption capacity of the diaphragm and the electrolyte, and improves the battery cycle rate performance. However, conventional ceramic coatings (such as aluminum oxide) can only improve the wettability of the diaphragm, and the ability to improve the ion transmission capacity of the diaphragm and the negative electrode interface is limited, resulting in the problem of low constant current charging ratio and negative lithium deposition at high rates.
[0004] In addition, the conventional inert ceramic coating and glue coating solutions for improving the high-temperature dimensional stability of the ion membrane cannot prevent the accumulation of heat in the battery and cause thermal runaway. According to the thermal runaway sequence, the ternary cathode material is very likely to undergo phase change under high temperature conditions and produce reactive oxygen with high chemical reactivity (broadly refers to free radicals and non-free radicals derived from oxygen, including superoxide anions (O2 - ), hydroxyl radical (•OH) and singlet oxygen ( 1 O2)). The exothermic reaction of active oxygen with the active electrolyte and the lithium-intercalated negative electrode is one of the main reasons for accelerating the thermal runaway of the battery.
[0005] Cerium oxide (CeO2) usually exists in the form of fluorite phase, with a face-centered cubic (fcc) crystal structure. Each cerium ion is coordinated with 8 oxygen ions, and the electronic structure of cerium (i.e. [Xe] 4f15d16s2) makes it 4+ and Ce 3+ Reversible charge transfer is easier between Ce 3+ The formation of ions is usually accompanied by the presence of oxygen vacancies on the surface and in the bulk, which is usually detected by XPS testing of Ce samples. 3+ / Ce atomic percentage to indirectly characterize the oxygen vacancy concentration of the material. 2-x It has the function of adsorbing anions and removing active oxygen, and is widely used to improve the cycle and rate performance of lithium-ion batteries.
[0006] Since the formation energy of oxygen vacancies in cerium oxide on the (111) crystal plane is low, oxygen vacancies mainly exist stably on the (111) crystal plane of the particles, and the reactivity of cerium oxide is closely related to the concentration of oxygen vacancies. Therefore, it is particularly important to regulate the structure, morphology and crystal plane of cerium oxide. The common method for regulating the morphology and exposed crystal plane type of nano-cerium oxide particles is hydrothermal / solvothermal method, with the assistance of surfactants or templates. However, since the hydrothermal / solvothermal method often uses toxic or expensive additives and surfactants to regulate the morphology of nano-cerium oxide, and requires high temperature, high pressure and long processing time, it cannot meet the actual needs of environmentally friendly preparation of nanomaterials; on the other hand, the new functional groups introduced in the preparation process of this method are not easy to be completely removed, which interferes with the performance of nano-cerium oxide and limits the practical application of nano-cerium oxide. Summary of the invention
[0007] In order to solve the above problems, the present invention provides a cerium oxide (111)-CeO with simple production process, low cost, high oxygen vacancy concentration and suitable for large-scale application. 2-x .
[0008] The present application provides a cerium oxide having oxygen vacancies, wherein the cerium oxide is (111)-CeO 2-x , where 0<X≤0.45, the (111)-CeO 2-x The surface has a (111) crystal plane.
[0009] The (111)-CeO 2-x The oxygen vacancy concentration is Rt, wherein 0<Rt≤90%, Rt is preferably 5%~60%, and more preferably 10%~40%.
[0010] Furthermore, the (111) crystal plane ratio is Rc, 10%≤Rc<100%, Rc is preferably greater than 30%, and more preferably greater than 50%.
[0011] Furthermore, in the (111)-CeO 2-x The retention rate of the oxygen vacancy concentration after storage at 55°C for 7 days is not less than 90%, preferably not less than 95%.
[0012] Furthermore, the (111)-CeO 2-x The D50 particle size is 50nm-2μm, preferably 100nm-1μm.
[0013] The present application also provides a method for preparing cerium oxide with specific oxygen vacancies, comprising the following steps:
[0014] Dispersing CeO2 in an acidic solution containing a reducing agent, stirring and dispersing the solution uniformly, and obtaining (111)-CeO2;
[0015] The (111)-CeO2 is deoxidized to obtain (111)-CeO 2-x , where 0<X≤0.45;
[0016] The (111)-CeO 2-x The oxygen vacancy concentration ratio is Rt, wherein 0<Rt≤90%, Rt is preferably 10%~70%, and more preferably 30%~60%.
[0017] Furthermore, the (111)-CeO2 preparation process comprises the following steps:
[0018] Dispersing CeO2 in acidic solution 1 and stirring evenly to obtain solution 1;
[0019] Dispersing the reducing agent in the acidic solution 2, and stirring evenly to obtain the solution 2;
[0020] The solution 2 is added to the solution 1 and stirred evenly to obtain (111)-CeO2.
[0021] Furthermore, the molar ratio of CeO2 to the reducing agent is 1:(0.01-10), preferably 1:(0.05-5).
[0022] Further, the concentration of the acidic solution 1 is 0.001-10 mol / L, preferably 1-6 mol / L; and / or
[0023] The concentration of the second acidic solution is 0.001-10 mol / L, preferably 1-6 mol / L; and / or
[0024] The concentration of the reducing agent in the second solution is 0.001-0.3 mol / L, preferably 0.01-0.05 mol / L.
[0025] Further, the reducing agent is selected from one of TiCl3, TiBr3, Ti2(SO4)3, and TiPO4; or
[0026] The acidic solution one and the acidic solution two are one of a hydrohalic acid solution, a sulfuric acid solution and a phosphoric acid solution.
[0027] Furthermore, the deoxidation treatment includes a vacuum deoxidation method, an inert atmosphere deoxidation method or a heating hydrogenation method.
[0028] Furthermore, (111)-CeO was prepared by this method. 2-x For the aforementioned (111)-CeO 2-x .
[0029] The present application also provides a composite diaphragm, comprising a diaphragm substrate and a functional coating coated on the surface of the diaphragm substrate, wherein the functional coating comprises the aforementioned (111)-CeO 2-x Or (111)-CeO prepared by the aforementioned method 2-x .
[0030] The present application provides a pole piece, comprising the aforementioned (111)-CeO 2-x Or (111)-CeO prepared by the aforementioned method 2-x .
[0031] The present application provides a (111)-CeO 2-x Or (111)-CeO prepared by the aforementioned method 2-x Application in lithium batteries.
[0032] The cerium oxide (111)-CeO with oxygen vacancies provided in this application 2-x , due to (111)-CeO 2-x The surface of the Ce 3+ The ions mainly exist on the (111) crystal plane, where Ce 3+ ions, so (111)-CeO 2-x There are many oxygen vacancies in the (111)-CeO. Since oxygen vacancies have the function of adsorbing anions and removing active oxygen, when the (111)-CeO 2-x When used in lithium batteries, it can effectively delay the degree of thermal runaway and improve the migration ability of lithium ions at the electrode electrolyte interface. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] The accompanying drawings are used to better understand the present application and do not constitute an improper limitation on the present application.
[0034] Figure 1 The cerium oxide (111)-CeO of Example 1 provided in this application 2-x TEM image of.
[0035] Figure 2 The cerium oxide (111)-CeO of Example 1 provided in this application 2-x TEM image of.
[0036] Figure 3 The cerium oxide (111)-CeO of Example 1 provided in this application 2-x TEM image of.
[0037] Figure 4 This is a TEM image of the cerium oxide of Comparative Example 5 provided in the present application. DETAILED DESCRIPTION
[0038] The following is a description of the exemplary embodiments of the present application, including various details of the embodiments of the present application to facilitate understanding, which should be considered as merely exemplary. Therefore, it should be recognized by those of ordinary skill in the art that various changes and modifications can be made to the embodiments described herein without departing from the scope and spirit of the present application. Similarly, for clarity and conciseness, the description of well-known functions and structures is omitted in the following description.
[0039] The first part of the present application provides a cerium oxide with oxygen vacancies, wherein the cerium oxide is (111)-CeO 2-x , where 0<X≤0.45.
[0040] Furthermore, the (111)-CeO 2-x The surface of CeO has a (111) crystal plane. 2-x The oxygen vacancy concentration is Rt, wherein 0<Rt≤90%, Rt is preferably 5% to 60%, and more preferably 10% to 40%. For example, Rt can be 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, etc.
[0041] The (111)-CeO 2-x The oxygen vacancy concentration Rt is the ratio of the number of defects left after oxygen escapes from the lattice position to the number of oxygen theoretically present in the lattice. The measurement method is: Ce 3+ The formation of ions is usually accompanied by the presence of oxygen vacancies on the surface and in the bulk, which is usually detected by XPS testing of Ce samples. 3+ The material to be tested is placed in an X-ray photoelectron spectrometer and an XPS test is performed after etching 10 nm. 3+ and Ce 4+ Electron combination, refine and separate the Ce element photoelectron peak, measure the peak area and calculate the atomic concentration. Oxygen vacancy concentration Rt (%) = Ce 3+ Peak area / (Ce 3+ Peak area + Ce 4+ Peak area)×100%.
[0042] In this paper, according to Rt=2x, the specific value of x can be calculated by the oxygen vacancy concentration Rt.
[0043] In the present application, the (111) crystal plane ratio is Rc, 10%≤Rc<100%, Rc is preferably 30% or more, and more preferably 50% or more. For example, Rc can be 10%, 15%, 20%, 5%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 96%, 97%, 98%, 99%, etc.
[0044] The (111)-CeO 2-x The (111) crystal plane ratio Rc is the area ratio of the (111) crystal plane on the material surface to all crystal planes. The measurement method is as follows: the material to be tested is placed in a transmission electron microscope to take a photo. The magnification of the electron microscope is set so that one particle enters the field of view. Each particle is measured as follows: Figure 1 The method shown in the figure selects 8 points and observes them at a magnification of 800k. Figure 2 The method shown measures the perimeter D1 of the 111 crystal plane and the perimeter D2 of other crystal planes, calculates the (111) crystal plane ratio Rc (%) = D1 / (D2+D1)×100 of the particle, and takes 5 particles to calculate the average value.
[0045] In this application, the (111)-CeO 2-x The retention rate of the oxygen vacancy concentration after storage at 55°C for 7 days is not less than 90%, preferably not less than 95%.
[0046] The oxygen vacancy concentration retention rate is the ratio of the oxygen vacancy concentration of the powder after being stored at 55°C for 7 days to that before being stored. The oxygen vacancy concentration retention rate % = (oxygen vacancy concentration after 7 days of high temperature storage at 55°C) / (initial oxygen vacancy concentration) * 100%.
[0047] In this application, the (111)-CeO 2-xThe D50 particle size is 50nm-2μm, preferably 100nm-1μm, for example, it can be 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 110nm, 120nm, 130nm, 140nm, 150nm, 160nm, 170nm, 180nm, 190nm, 200nm, 210nm, 220nm, 230nm, 240nm, 250nm, 260nm, 270nm, 280nm, 290nm, 300nm, 310nm, 320nm, 330nm, 340nm, 350nm, 360nm, 370nm, 380nm, 390nm, 400nm, 450nm, 500nm, 550nm, 600nm, 650nm, 700nm, 750nm , 800nm, 850nm, 900nm, 1000nm, 1100nm, 1200nm, 1300nm, 1400nm, 1500nm, 1600nm, 1700nm, 1800nm, 1900nm, 2000nm.
[0048] In this article, the D50 particle size is the particle size D50 of the dispersion tested using a laser particle size analyzer. The solvent in the test injector is deionized water. The powder to be tested is dispersed in the solvent by ultrasound or mechanical stirring, and the sample is dripped into the test injector for testing. The diameter of the particles that account for 50% of the volume of the sample is the D50 value. The test parameters are set as follows: the material refractive index is 2.42, the absorptivity is 1.0, and the shading degree is 1-4%.
[0049] In this application, the (111)-CeO 2-x The superoxide anion clearance rate is greater than or equal to 50%. For example, it can be 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59%, 60%, 61%, 62%, 63%, 64%, 65%, 66%, 67%, 68%, 69%, 70%, 71%, 72%, 73%, 74%, 75%, etc.
[0050] The superoxide anion clearance rate was determined as follows:
[0051] ① Prepare the DMSO solution of nitro blue tetrazolium chloride (NBT) by drying and pyrogallol aqueous solution, and store in dark for later use;
[0052] ② Take pyrogallol solution, phosphate buffer and deionized water in a black cap bottle in a ratio of 1:3:6, mix them evenly, and directly shake them in the dark for 10 minutes as the blank group. Add the powder to be tested and shake them in the dark for 1 minute as the experimental group;
[0053] ③ Filter the suspension after the reaction, weigh the mass of the precipitate, divide the mass of the precipitate by the mass of the blank group precipitate, and evaluate the clearance rate.
[0054] The second part of this application provides a method for preparing cerium oxide with a specific surface, comprising the following steps:
[0055] Step 1: Acid treatment
[0056] Dispersing CeO2 in an acidic solution containing a reducing agent, stirring and dispersing the solution uniformly, and obtaining (111)-CeO2;
[0057] Step 2: Deoxidation treatment
[0058] The (111)-CeO2 is deoxidized to obtain (111)-CeO 2-x , where 0<X≤0.45; the (111)-CeO 2-x The surface of CeO has a (111) crystal plane. 2-x The oxygen vacancy concentration is Rt, wherein 0<Rt≤90%, Rt is preferably 5%~60%, and more preferably 10%~40%.
[0059] In step 1, the (111)-CeO2 preparation process specifically includes the following steps:
[0060] Step 1.1: Disperse CeO2 in acidic solution 1 and stir to obtain solution 1;
[0061] Step 1.2: Disperse the reducing agent in the acidic solution 2, and stir evenly to obtain the solution 2;
[0062] Step 1.3: Slowly add the solution 2 into the solution 1 and stir evenly to obtain (111)-CeO2.
[0063] The D50 particle size of the CeO2 is 50nm-2μm, preferably 100nm-1μm, for example, 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 110nm, 120nm, 130nm, 140nm, 150nm, 160nm, 170nm, 180nm, 190nm, 200nm, 210nm, 220nm, 230nm, 240nm, 250nm, 260nm, 270nm, 280nm, 290nm, 300nm, 310nm nm, 320nm, 330nm, 340nm, 350nm, 360nm, 370nm, 380nm, 390nm, 400nm, 450nm, 500nm, 550nm, 600nm, 650nm, 700nm, 750n m, 800nm, 850nm, 900nm, 1000nm, 1100nm, 1200nm, 1300nm, 1400nm, 1500nm, 1600nm, 1700nm, 1800nm, 1900nm, 2000nm.
[0064] The molar ratio of CeO2 to the reducing agent is 1:(0.01~10), preferably 1:(0.05~5), for example, it can be 1:0.01, 1:0.05, 1:0.08, 1:0.1, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5, 1:6, 1:6.5, 1:7, 1:7.5, 1:8, 1:8.5, 1:9, 1:9.5, 1:10, etc.
[0065] The concentration of the acidic solution one or the concentration of the acidic solution two is 0.001-10 mol / L, preferably 1-6 mol / L, for example, 0.005 mol / L, 0.01 mol / L, 0.05 mol / L, 0.1 mol / L, 0.5 mol / L, 1 mol / L, 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L, 4 mol / L, 4.5 mol / L, 5 mol / L, 5.5 mol / L, 6 mol / L, 6.5 mol / L, 7 mol / L, 7.5 mol / L, 8 mol / L, 8.5 mol / L, 9 mol / L, 9.5 mol / L, 10 mol / L, etc.
[0066] Too high concentrations of acid solution 1 and acid solution 2 will lead to more corrosion of CeO2 and reduced yield. In addition, it will also cause corrosion of equipment. Even higher concentrations of acid will pose a safety hazard. Too low a concentration will lead to a low proportion of (111) crystal planes on the CeO2 surface, which will in turn affect the oxygen vacancy concentration.
[0067] The molar ratio of CeO2 in the solution 1 to the acid in the acidic solution 1 is 1:(0.1~20), preferably 1:(5~10), for example, it can be 1:0.1, 1:0.5, 1:1, 1:1.5, 1:2, 1:2.5, 1:3, 1:3.5, 1:4, 1:4.5, 1:5, 1:5.5, 1:6, 1:6.5, 1:7, 1:7.5, 1:8, 1:8.5, 1:9, 1:9.5, 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, 1:16, 1:17, 1:18, 1:19, 1:20, etc.
[0068] The concentration of the reducing agent in the second solution is 0.001-0.3 mol / L, preferably 0.01-0.05 mol / L, for example, 0.001 mol / L, 0.005 mol / L, 0.01 mol / L, 0.02 mol / L, 0.03 mol / L, 0.04 mol / L, 0.05 mol / L, 0.06 mol / L, 0.07 mol / L, 0.08 mol / L, 0.09 mol / L, 0.1 mol / L, 0.2 mol / L, 0.3 mol / L, etc. If the concentration of the reducing agent in the second solution is too high, the chemical stability of the CeO2 (111) crystal plane will be reduced and the reducing agent will be wasted. If the concentration is too low, the reducibility will be reduced and the proportion of the (111) crystal plane on the CeO2 surface will be low.
[0069] The reducing agent is selected from one of TiCl3, TiBr3, Ti2(SO4)3, and TiPO4.
[0070] The acidic solution one and the acidic solution two are one of a hydrohalic acid solution, a sulfuric acid solution and a phosphoric acid solution.
[0071] The acids in the acidic solution 1 and the acidic solution 2 are preferably the same type of acid.
[0072] The hydrohalic acid may be HCl, HBr or HI.
[0073] In some embodiments, the acidic solution 2 and the reducing agent have the same anion.
[0074] In some embodiments, the second acidic solution is HCl solution, and the reducing agent is TiCl3.
[0075] In some embodiments, the second acidic solution is a HBr solution, and the reducing agent is TiBr3.
[0076] In some embodiments, the acidic solution is a sulfuric acid solution, and the reducing agent is Ti2(SO4)3.
[0077] In step 2, the (111)-CeO2 is deoxidized by vacuum deoxidation, inert atmosphere deoxidation or heating hydrogenation to obtain (111)-CeO 2-x .
[0078] Specifically, when the vacuum deoxidation method is adopted, the specific steps are as follows:
[0079] Step 2a: placing (111)-CeO2 in a reaction chamber, and evacuating the reaction chamber by a vacuum pump until the vacuum degree in the reaction chamber reaches -80 kPa to -99 kPa;
[0080] Step 2b: repeatedly introducing an inert gas into the reaction chamber, and then evacuating the reaction chamber by a vacuum pump to clean the reaction chamber;
[0081] Step 2c: evacuate the reaction chamber by a vacuum pump until the pressure in the reaction chamber reaches -99 kPa~-100 kPa; turn on the heating device to heat to a preset temperature, and continue the reaction to prepare (111)-CeO 2-x .
[0082] The preset temperature is 400-1800°C, preferably 800-1200°C, for example, it can be 400°C, 500°C, 600°C, 700°C, 800°C, 900°C, 1000°C, 1100°C, 1200°C, 1300°C, 1400°C, 1500°C, 1600°C, 1700°C, 1800°C, etc.
[0083] The reaction time at the preset temperature is 0 to 48 h, preferably 2 to 12 h, for example, 2 h, 4 h, 8 h, 10 h, 12 h, 14 h, 16 h, 18 h, 20 h, 22 h, 24 h, 26 h, 28 h, 30 h, 32 h, 34 h, 36 h, 38 h, 40 h, 42 h, 44 h, 46 h, 48 h, etc.
[0084] Specifically, when the inert atmosphere deoxidation method is adopted, the specific steps are as follows:
[0085] Step 2a: placing (111)-CeO2 in a reaction chamber, and evacuating the reaction chamber by a vacuum pump until the vacuum degree in the reaction chamber reaches -80 kPa to -99 kPa;
[0086] Step 2b: repeatedly introducing an inert gas into the reaction chamber, and then evacuating the reaction chamber by a vacuum pump to clean the reaction chamber;
[0087] Step 2c: Introduce an inert gas into the reaction chamber until the pressure in the reaction chamber reaches 101 kPa, turn on the heating device to heat to a preset temperature, and continue the reaction to prepare (111)-CeO 2-x .
[0088] The inert gas includes but is not limited to nitrogen, argon, and helium.
[0089] The preset temperature is 400-1800°C, preferably 800-1200°C, for example, it can be 400°C, 500°C, 600°C, 700°C, 800°C, 900°C, 1000°C, 1100°C, 1200°C, 1300°C, 1400°C, 1500°C, 1600°C, 1700°C, 1800°C, etc.
[0090] The reaction time at the preset temperature is 0 to 48 h, preferably 2 to 12 h, for example, 1 h, 2 h, 4 h, 8 h, 10 h, 12 h, 14 h, 16 h, 18 h, 20 h, 22 h, 24 h, 26 h, 28 h, 30 h, 32 h, 34 h, 36 h, 38 h, 40 h, 42 h, 44 h, 46 h, 48 h, etc.
[0091] Specifically, when the heating hydrogenation method is adopted, the specific steps are as follows:
[0092] Step 2a: placing (111)-CeO2 in a reaction chamber, and evacuating the reaction chamber by a vacuum pump until the vacuum degree in the reaction chamber reaches -80 kPa to -99 kPa;
[0093] Step 2b: repeatedly introducing an inert gas into the reaction chamber, and then evacuating the reaction chamber by a vacuum pump to clean the reaction chamber;
[0094] Step 2c: A hydrogen-argon mixed gas is introduced into the reaction chamber until the pressure in the reaction chamber reaches 101 kPa, and a heating device is turned on to heat the reaction chamber to a preset temperature, and the reaction is continued to prepare (111)-CeO 2-x .
[0095] The hydrogen-argon mixed gas accounts for 5%-95%.
[0096] The preset temperature is 400-1800°C, preferably 800-1200°C, for example, it can be 400°C, 500°C, 600°C, 700°C, 800°C, 900°C, 1000°C, 1100°C, 1200°C, 1300°C, 1400°C, 1500°C, 1600°C, 1700°C, 1800°C, etc.
[0097] The reaction time at the preset temperature is 0 to 48 h, preferably 2 to 12 h, for example, 1 h, 2 h, 4 h, 8 h, 10 h, 12 h, 14 h, 16 h, 18 h, 20 h, 22 h, 24 h, 26 h, 28 h, 30 h, 32 h, 34 h, 36 h, 38 h, 40 h, 42 h, 44 h, 46 h, 48 h, etc.
[0098] In the present application, (111)-CeO is prepared by the preparation method described in the present application. 2-x For the aforementioned (111)-CeO 2-x , its various parameters can refer to the above description.
[0099] The present application also provides a composite diaphragm, comprising a diaphragm substrate and a functional coating coated on the surface of the diaphragm substrate, wherein the functional coating comprises the aforementioned (111)-CeO 2-x Or (111) CeO prepared by the aforementioned method 2-x .
[0100] In some embodiments, the functional coating is (111)-CeO 2-x The layer has a thickness of 0.1-10 μm, for example, 0.1 μm, 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, or 10 μm.
[0101] The separator substrate includes, but is not limited to, a polyester polyolefin porous membrane, and a polyolefin porous membrane loaded with alumina or boehmite on one or both sides.
[0102] The present application also provides a pole piece, which includes the aforementioned (111)-CeO 2-x Or (111)-CeO prepared by the above method 2-x .
[0103] In some embodiments, the pole piece includes a pole piece body and a coating applied on the surface of the pole piece body, wherein the coating contains the aforementioned (111)-CeO 2-x Or (111)-CeO prepared by the aforementioned method 2-x .
[0104] In some embodiments, the pole piece includes a pole piece substrate, wherein the pole piece substrate is mixed with the aforementioned (111)-CeO 2-x Or (111)-CeO prepared by the aforementioned method 2-x .
[0105] Contains (111)-CeO 2-xThe coating material can be used in the fields of membrane surface coating, positive and negative electrode mixing and pole piece surface coating, without changing the current mainstream battery preparation process. It has the advantages of high stability and low cost and is suitable for large-scale application. Moreover, compared with the positive electrode surface coating method, the (111)-CeO 2-x When the coating material is coated on the surface of the diaphragm / pole piece, the load capacity is larger, the functional surface continuity is better, the process is simpler and low-cost, and the material is not easily oxidized under high voltage at the positive electrode.
[0106] The (111)-CeO 2-x It can be used in lithium batteries. 2-x The (111) crystal plane accounts for a large proportion of the surface, so the (111)-CeO 2-x It has a large amount of trivalent cerium and oxygen vacancies. When used in lithium batteries, it can capture active oxygen in the battery cycle through charge action, especially active oxygen generated by the positive electrode under extreme abnormal working conditions such as hot box or overcharge, thereby preventing the exothermic redox reaction between active oxygen and negative electrode active materials, thereby avoiding continuous temperature rise inside the battery cell and causing thermal runaway. In addition, due to the (111)-CeO 2-x There is a lack of oxygen ions in the crystal lattice, so the exposed positively charged metal ions can adsorb the anions in the lithium salt and promote the dissociation of the lithium salt.
[0107] The preferred method for regulating the morphology and exposed crystal face type of nano-cerium oxide particles in the current prior art is the hydrothermal / solvothermal method, which, with the assistance of surfactants or templates, has a simple process, low cost and is suitable for large-scale applications compared to the preparation method described in this application.
[0108] Examples and Test Section
[0109] The experimental methods used in the following examples are all conventional methods unless otherwise specified.
[0110] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0111] Unless otherwise specified, the acidic solution 1 and the acidic solution 2 in the following embodiments are of the same acid and concentration and are collectively referred to as acidic solutions.
[0112] 1. Implementation
[0113] Example 1
[0114] Step 1: Disperse CeO2 with a particle size D50 of 400 nm in 5 mol / L HCl acidic solution 1 and stir to disperse evenly. Under continuous stirring, add 0.02 mol / L TiCl3 in HCl (5 mol / L) solution dropwise, react for 5 minutes, and finally filter, wash and dry the treated dispersion to obtain the treated (111)-CeO2. The molar ratio of CeO2: HCl: TiCl3 in the acidic solution 1 is 1:5:0.2, and the acid treatment reduction time is 5 minutes to obtain (111)-CeO2.
[0115] Step 2:
[0116] Step 2a: Place (111)-CeO2 in a reaction chamber, and evacuate the reaction chamber using a vacuum pump until the vacuum degree in the reaction chamber reaches -99 kPa.
[0117] Step 2b: repeatedly introducing an inert gas into the reaction chamber, and then evacuating the reaction chamber by a vacuum pump to clean the reaction chamber.
[0118] Step 2c: A 5% hydrogen-argon mixed gas was introduced into the reaction chamber. When the pressure reached 101 kPa, the heating device was turned on to heat the reaction chamber to 500 °C and the reaction was continued for 2 min to prepare (111)-CeO 2-x .
[0119] (111)-CeO prepared by the above method 2-x , used to test material properties, among which the superoxide anion scavenging activity test results are shown in Table 1, (111)-CeO 2-x TEM images at different magnifications are shown in Figure 1-Figure 3 .
[0120] Step 3: Take 1 part by weight of dispersant sodium polyacrylate and add it to 2000 parts by weight of water, stir thoroughly, and then add 100 parts by weight of (111)-CeO 2-x The (111)-CeO 2-x The particles were uniformly dispersed to a particle size D50 of 400 nm, and then 1 part by weight of a thickener, sodium carboxymethyl cellulose, 5 parts by weight of a binder, polyacrylate, and 0.4 parts by weight of a wetting agent, sodium perfluorooctanoate, were added and stirred thoroughly to obtain a coating slurry;
[0121] Step 4: Take the coating slurry and apply it on the diaphragm substrate through a micro-gravure coating machine, bake it at 40° C. for 2 minutes to form a functional layer, and roll it up to obtain the composite diaphragm.
[0122] The diaphragm substrate is a polyethylene film with aluminum oxide coating on both sides, wherein the thickness of the aluminum oxide coating is 2 μm and the thickness of the polyethylene film is 9 μm; (111)-CeO2-x The coating thickness is 2 μm;
[0123] The lithium battery composite separator prepared by the above method was used to assemble a lithium battery. The battery structure was a NCM83||SiOC450 soft-pack battery. The (111)-CeO2-x coating faced the positive electrode side. Lithium hexafluorophosphate-LiFSI polyester electrolyte was used to assemble the soft-pack battery cell for testing. The specific performance test results are shown in Table 1.
[0124] The difference between Example 2 and Example 3 and Example 1 is that in step 3, the (111)-CeO 2-x The particles are evenly dispersed into particles with different particle sizes D50. Other parameters are shown in Table 1.
[0125] The difference between Example 4 and Example 5 and Example 1 is that the concentration of TiCl3 in step 1 is different. Other parameters are shown in Table 2.
[0126] The difference between Example 6 to Example 8 and Example 1 is that the concentration of the HCl acid solution in step 1 is different. Other parameters are shown in Table 3.
[0127] The difference between Example 9 and Example 10 is that the type of the acid solution in step 1 is different. The other parameters are shown in Table 4.
[0128] The difference between Example 11 to Example 13 and Example 1 is that the type of atmosphere in step 2c is different. Other parameters are shown in Table 5.
[0129] The difference between Comparative Example 1 and Comparative Example 2 and Example 1 is that the concentration of TiCl3 in step 1 is different. Other parameters are shown in Table 2.
[0130] The difference between Comparative Example 3 and Example 1 is that the concentration of the HCl acid solution in step 1 is different. Other parameters are shown in Table 3.
[0131] The difference between Comparative Example 4 and Example 1 is that the type of atmosphere in step 2c is different. Other parameters are shown in Table 5.
[0132] The difference between Comparative Example 5 and Example 1 is that there is no step 1 and step 2, that is, CeO2 is not treated. Other parameters are shown in Table 6 and the TEM image of CeO2 is shown in Figure 4 ,Depend on Figure 4 It can be seen that CeO2 mainly consists of (200) crystal plane.
[0133] The only difference between Comparative Example 6 and Example 1 is that there is no step 2. Other parameters are shown in Table 6.
[0134] The difference between Comparative Example 7 and Example 1 is that there is no step 1. Other parameters are shown in Table 6.
[0135] The only difference between Comparative Example 8 and Example 1 is that the composite separator of the lithium battery is a polyethylene film with aluminum oxide coating on both sides, wherein the thickness of the aluminum oxide coating is 2 μm and the thickness of the polyethylene film is 9 μm. See Table 6 for other parameters.
[0136] 2. Test part
[0137] 1. Test method:
[0138] 1. The method for determining the overcharge pass rate is as follows:
[0139] The battery is discharged at a constant current to the discharge cut-off voltage, and then charged at a constant current of 3C rate or 3 times the manufacturer's recommended charging current, whichever is greater, to 160% SOC, and then left to stand for 1 hour. The battery has passed if it does not catch fire or explode.
[0140] 2. The method for determining the hot box pass rate is as follows:
[0141] The battery is first discharged at a constant current to the discharge cut-off voltage, and then charged at a constant current to a fully charged state, and then placed in a test chamber. The test chamber is heated at a temperature rise rate of 5°C / min. When the temperature in the chamber reaches 140°C±2°C, the temperature is kept constant for 1 hour, and then the temperature is raised at a temperature rise rate of 5°C / min. When the temperature in the chamber reaches 150°C±2°C, the temperature is kept constant for 1 hour, and then the temperature is raised at a temperature rise rate of 5°C / min. When the temperature in the chamber reaches 160°C±2°C, the temperature is kept constant for 1 hour. During the whole process, the battery should not catch fire or explode, which means it has passed.
[0142] 3. The room temperature cycle life is determined as follows:
[0143] a) Discharge at 1C current to the material discharge termination voltage at 23℃±2℃, and let stand for 1h;
[0144] b) Charge at 1C current to the material charging termination voltage, then switch to constant voltage charging until the charging current rate drops to 0.05C, and let stand for 1 hour;
[0145] c) The battery is discharged at 1C current to the material discharge termination voltage, and the discharge specific capacity is recorded;
[0146] d) Repeat steps a and b three times, and select the average of the discharge capacity of the three tests as the initial capacity; the battery is continuously charged and discharged at a current of 1C. If the discharge capacity is lower than 80% of the initial capacity, the test is terminated, and the total number of weeks during which the capacity is higher than the initial capacity is recorded.
[0147] 4. The determination method of 3C constant current charging ratio is as follows:
[0148] a) Discharge at 0.33C current to the material discharge termination voltage at 23℃±2℃, and let stand for 1h;
[0149] b) Charge at 3C current until the material charging termination voltage is reached, then switch to constant voltage charging until the charging current rate drops to 0.05C, and let stand for 1 hour;
[0150] c) The battery is discharged at a current of 0.33C to the material discharge termination voltage, and the discharge specific capacity is recorded;
[0151] d) 3C constant current charging ratio = 3C constant current charging capacity / (3C constant current charging capacity + termination voltage constant voltage charging capacity)*100;
[0152] e) Repeat steps b and c three times and record the average value of the 3C constant current charging ratio of the three tests.
[0153] (II) Test results of various embodiments
[0154] 1. Table 1 is (111)-CeO 2-x Effect of different particle size D50
[0155] .
[0156] 2. Table 2 shows the effects of different TiCl3 concentrations in solution 2
[0157] .
[0158] 3. Table 3 shows the effects of different concentrations of acidic solutions
[0159] .
[0160] 4. Table 4 shows the effects of different types of acid when the same acid solution is added twice in step 1.
[0161] .
[0162] 5. Table 5 shows the effects of different gas types in step 2
[0163] .
[0164] 6. Table 6 is a comparison of each comparative example with Example 1
[0165] .
[0166] It can be seen from Tables 1-6 that (111)-CeO prepared by the method of the present application 2-xThe invention has strong superoxide ion scavenging performance when applied to lithium batteries, and the lithium batteries have the characteristics of high safety, good battery performance and high stability. When CeO2 is used directly or only subjected to acid treatment and applied to lithium batteries, since CeO2 has fewer trivalent cerium ions and fewer oxygen vacancies, its superoxide ion scavenging effect is poor, resulting in poor battery performance of the lithium battery. When CeO2 is subjected to acid treatment and reduced or CeO2 is directly calcined and applied to lithium batteries, only a small portion of tetravalent cerium is reduced to trivalent cerium, so the battery performance and safety of the lithium battery are still low.
[0167] Although the embodiments of the present application are described above in conjunction with the accompanying drawings, the present application is not limited to the above specific embodiments and application fields, and the above specific embodiments are merely illustrative and instructive, rather than restrictive. A person of ordinary skill in the art can also make many forms under the guidance of this specification and without departing from the scope of protection of the claims of the present application, all of which belong to the protection of the present application.
Claims
1. A composite separator for a lithium battery, wherein: The invention comprises a membrane substrate and a functional coating coated on the surface of the membrane substrate, wherein the functional coating comprises (111)-CeO 2-x , where 0<X≤0.45, the (111)-CeO 2-x The surface of the (111)-CeO has a (111) crystal plane; the (111) crystal plane accounts for Rc, and Rc is greater than 28.4% and less than 100%. 2-x The retention rate of oxygen vacancy concentration in the atmosphere after storage at 55°C for 7 days is not less than 90%.
2. The composite separator of a lithium battery according to claim 1, wherein: The (111)-CeO 2-x The oxygen vacancy concentration is Rt, where 0<Rt≤90%.
3. The composite separator of a lithium battery according to claim 2, wherein: The Rt is 5% to 60%.
4. The composite separator of a lithium battery according to claim 2, wherein: The Rt is 10%~40%.
5. The composite separator of a lithium battery according to any one of claims 1 to 4, wherein: The Rc is greater than 30%.
6. The composite separator of a lithium battery according to any one of claims 1 to 4, wherein: The Rc is greater than 50%.
7. The composite separator of a lithium battery according to claim 5, wherein: In the (111)-CeO 2-x The retention rate of oxygen vacancy concentration in the sample after storage in a high temperature atmospheric environment of 55°C for 7 days is not less than 95%.
8. The composite separator of a lithium battery according to any one of claims 1 to 2, wherein: The (111)-CeO 2-x The D50 particle size is 50nm-2μm.
9. The composite separator of a lithium battery according to any one of claims 1 to 2, wherein: The (111)-CeO 2-x The D50 particle size is 100nm-1μm.
10. A method for preparing cerium oxide having oxygen vacancies, wherein: The steps include: Dispersing CeO2 in acidic solution 1 and stirring evenly to obtain solution 1; Dispersing the reducing agent in the acidic solution 2, and stirring evenly to obtain the solution 2; Adding the solution 2 into the solution 1 and stirring evenly to obtain (111)-CeO2; The (111)-CeO2 is deoxidized to obtain (111)-CeO 2-x , where 0<X≤0.45; The concentration of the acidic solution 1 is 0.001-10 mol / L; The concentration of the second acidic solution is 0.001-10 mol / L; The concentration of the reducing agent in the second solution is 0.001-0.3 mol / L; The (111)-CeO 2-x The surface of the (111)-CeO 2-x The retention rate of oxygen vacancy concentration in the atmosphere after storage at 55°C for 7 days is not less than 90%.
11. The preparation method according to claim 10, wherein: The concentration of the acidic solution 1 is 1-6 mol / L; and / or The concentration of the second acidic solution is 1-6 mol / L; and / or The concentration of the reducing agent in the second solution is 0.01-0.05 mol / L.
12. The preparation method according to claim 10, wherein: The reducing agent is selected from one of TiCl3, TiBr3, Ti2(SO4)3, and TiPO4; and / or The acidic solution 1 and the acidic solution 2 are one of a hydrohalic acid solution, a sulfuric acid solution, and a phosphoric acid solution; and / or the deoxidation treatment comprises: a vacuum deoxidation method, an inert atmosphere deoxidation method, or a heating hydrogenation method to obtain (111)-CeO 2-x .
13. The preparation method according to claim 10, wherein: The (111)-CeO 2-x The oxygen vacancy concentration is Rt, where 0<Rt≤90%.
14. The preparation method according to claim 13, wherein: The Rt is 5% to 60%.
15. The preparation method according to claim 13, wherein: The Rt is 10%~40%.
16. The preparation method according to any one of claims 10 to 14, wherein: The Rc is greater than 30%.
17. The preparation method according to any one of claims 10 to 14, wherein: The Rc is greater than 50%.
18. The preparation method according to claim 16, wherein: In the (111)-CeO 2-x The retention rate of oxygen vacancy concentration in the sample after storage in a high temperature atmospheric environment of 55°C for 7 days is not less than 95%.
19. The preparation method according to any one of claims 10 to 14, wherein: The (111)-CeO 2-x The D50 particle size is 50nm-2μm.
20. The preparation method according to any one of claims 10 to 14, wherein: The (111)-CeO 2-x The D50 particle size is 100nm-1μm.
21. A pole piece, wherein: (111)-CeO prepared by the method according to any one of claims 10 to 20 2-x .
22. A composite separator for a lithium battery, wherein: The invention comprises a membrane substrate and a functional coating coated on the surface of the membrane substrate, wherein the functional coating comprises (111)-CeO prepared by the method according to any one of claims 10 to 20. 2-x .
23. A (111)-CeO prepared by the method according to any one of claims 10 to 20 2-x Application in lithium batteries.