Methods for catalyst preparation, and methods for catalyst and catalytic dehydrogenation of organic liquid hydrogen storage materials.

The catalyst was prepared by co-precipitation of nickel, magnesium, aluminum, rare earth and transition metal elements, which solved the problems of high cost and insufficient activity of dehydrogenation catalysts for organic liquid hydrogen storage materials. It achieved high efficiency, economical catalytic performance and stability, and is suitable for dehydrogenation reactions of various organic liquid hydrogen storage materials.

CN118437339BActive Publication Date: 2026-11-17YANCHENG HAIWANG HYDROGEN ENERGY TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410577213.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-10
Publication Date
2026-11-17
Estimated Expiration
2044-05-10

AI Technical Summary

Technical Problem

Existing organic liquid hydrogen storage materials have high cost, insufficient activity and poor selectivity in their dehydrogenation catalysts. Pt/Al2O3 catalysts are prone to coking and deactivation, and the use of precious metals is uneconomical.

Method used

The catalyst was prepared by co-precipitation of nickel, magnesium, aluminum, rare earth and transition metal elements. By controlling the chemical composition ratio and pH value, a stable hydrotalcite precursor structure was formed, which ensured the ultra-high dispersion of metal elements and avoided the use of precious metals.

Benefits of technology

It improves the activity, selectivity and thermal stability of the catalyst, reduces the preparation cost, solves the problem of easy catalyst deactivation, and is suitable for the dehydrogenation reaction of a variety of organic liquid hydrogen storage materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004832789400000141
    Figure BDA0004832789400000141
  • Figure BDA0004832789400000151
    Figure BDA0004832789400000151
Patent Text Reader

Abstract

This invention relates to the field of catalyst preparation technology, and discloses a method for preparing a catalyst, a catalyst, and a method for catalytic dehydrogenation of organic liquid hydrogen storage materials. The preparation method includes (1) mixing a precursor solution containing a nickel source, a magnesium source, an aluminum source, and a rare earth source with a precipitant under stirring conditions to carry out a first coprecipitation reaction to obtain a first suspension; (2) mixing a transition metal source, an alkali, and a solvent to carry out a second coprecipitation reaction to obtain a second suspension; the transition metal in the transition metal source includes zirconium and optionally chromium; (3) mixing the first suspension and the second suspension, and then performing an aging treatment to obtain a catalyst precursor; (4) calcining the catalyst precursor. The catalyst prepared by the above method can exhibit good catalytic activity, selectivity, anti-carbon deposition, and stability under relatively mild reaction conditions, while taking into account both high catalytic activity and excellent thermal stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of catalyst preparation technology, specifically to a method for preparing a catalyst, a catalyst, and a method for catalyzing the dehydrogenation of organic liquid hydrogen storage materials. Background Technology

[0002] Hydrogen energy is widely used in aerospace, civil applications, transportation, construction, energy storage, and other fields. It will become the mainstream direction of global energy development and play an important role in the energy transition system as an important component of the future sustainable and carbon-neutral energy society.

[0003] Currently, the most researched hydrogen storage methods can be broadly categorized into high-pressure hydrogen storage, liquid hydrogen storage, solid-state hydrogen storage, and organic liquid hydrogen storage. Organic liquid hydrogen storage technology involves reacting unsaturated organic matter with hydrogen under specific conditions to generate hydrogenation products, which are then stored as hydrogen. The hydrogen release stage involves releasing hydrogen through a catalytic dehydrogenation reaction. Based on reversible catalytic dehydrogenation reactions, N-ethylcarbazole (NEC), toluene, dibenzyltoluene (DBT), naphthalene, and other compounds can be utilized to achieve hydrogen energy utilization.

[0004] Currently, Pt / Al₂O₃ is commonly used as a dehydrogenation catalyst in organic liquid hydrogen storage technology, obtained through traditional impregnation or precipitation methods. Pt / Al₂O₃, as a catalyst with good selectivity and high conversion rate, is the most commonly used catalytic system in the dehydrogenation reaction of methylcyclohexane. However, Al₂O₃ contains many acidic sites, causing Pt particles to easily aggregate into larger particles, leading to catalyst deactivation due to coking and deposition. Furthermore, the extensive use of precious metals is detrimental to reducing process costs. Therefore, the development and preparation of highly efficient catalysts is crucial for the widespread adoption of novel organic liquid hydrogen storage systems. Summary of the Invention

[0005] The purpose of this invention is to overcome the problems of high cost, insufficient catalyst activity, and poor selectivity in the dehydrogenation of organic liquid hydrogen storage materials in the prior art. This invention provides a method for preparing a catalyst, a catalyst, and a method for catalyzing the dehydrogenation of organic liquid hydrogen storage materials. The preparation method uses relatively inexpensive raw materials, has a simple process, and produces a catalyst with high catalytic activity and good selectivity.

[0006] To achieve the above objectives, the present invention provides a method for preparing a catalyst, comprising the following steps:

[0007] (1) Under stirring conditions, a precursor solution containing nickel source, magnesium source, aluminum source and rare earth source is mixed with a precipitant to carry out a first coprecipitation reaction to obtain a first suspension; the pH of the first suspension is 5-8.

[0008] (2) A second coprecipitation reaction is carried out by mixing a transition metal source, an alkali and a solvent to obtain a second suspension; the pH of the second suspension is 4-7; the transition metal in the transition metal source includes zirconium and optionally chromium;

[0009] The total molar amount of nickel source (calculated as Ni) and magnesium source (calculated as Mg) is denoted as M1, the total molar amount of aluminum source (calculated as Al) and rare earth source (calculated as rare earth element) is denoted as M2, and the molar amount of transition metal source (calculated as transition metal element) is denoted as M3. The ratio of M1:M2:M3 is (2-4):1:(0.025-0.07).

[0010] (3) Mix the first suspension with the second suspension and then perform an aging treatment to obtain the catalyst precursor;

[0011] (4) The catalyst precursor is calcined.

[0012] Preferably, the pH of the second suspension is 1-2 lower than the pH of the first suspension.

[0013] A second aspect of the present invention provides a catalyst prepared by the above-described preparation method.

[0014] A third aspect of the present invention provides a method for catalytic dehydrogenation of an organic liquid hydrogen storage material, the method comprising: contacting the organic liquid hydrogen storage material with a dehydrogenation catalyst under dehydrogenation reaction conditions;

[0015] The dehydrogenation catalyst is the catalyst described in the second aspect.

[0016] Preferably, the organic liquid hydrogen storage material is selected from at least one of methylcyclohexane, tetrahydronaphthalene, decahydronaphthalene, perhydroN-ethylcarbazole, and perhydrocarbazole.

[0017] This invention effectively improves the utilization efficiency of catalyst preparation raw materials by strictly controlling the ratio of divalent metals (nickel and magnesium) to trivalent metals (aluminum and rare earth elements) in the chemical composition, and strictly controlling the pH value of the solution during precipitation. After aging treatment, a precursor with a stable composition and complete crystal structure with hydrotalcite structure is obtained. Moreover, in this precursor, various metal elements are atomically dispersed, which ensures the ultra-high dispersion and utilization efficiency of each component element in the catalyst finally obtained by this invention, further improving the activity of the catalyst.

[0018] Meanwhile, the catalyst provided by this invention does not require the introduction of precious metal components, which helps to reduce the catalyst preparation cost. Through the synergistic effect of Ni, Mg, Al, rare earth elements, and transition metal elements, the catalyst finally prepared by this invention for the dehydrogenation of organic liquid hydrogen storage materials can achieve both high catalytic activity and excellent thermal stability. In particular, the catalyst prepared by the method provided by this invention can exhibit good catalytic activity, selectivity, anti-coking, and stability under relatively mild reaction conditions, solving the problems of easy deactivation and short catalytic life cycle of similar catalysts. Moreover, the raw materials are economical and readily available, the preparation process is simple, and it has broad application prospects. Detailed Implementation

[0019] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of the various ranges, the endpoint values ​​of the various ranges and individual point values, and individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed herein.

[0020] The first aspect of this invention provides a method for preparing a catalyst, comprising the following steps:

[0021] (1) Under stirring conditions, a precursor solution containing nickel source, magnesium source, aluminum source and rare earth source is mixed with a precipitant to carry out a first coprecipitation reaction to obtain a first suspension; the pH of the first suspension is 5-8.

[0022] (2) A second coprecipitation reaction is carried out by mixing a transition metal source, an alkali and a solvent to obtain a second suspension; the pH of the second suspension is 4-7; the transition metal in the transition metal source includes zirconium and optionally chromium;

[0023] The total molar amount of nickel source (calculated as Ni) and magnesium source (calculated as Mg) is denoted as M1, the total molar amount of aluminum source (calculated as Al) and rare earth source (calculated as rare earth element) is denoted as M2, and the molar amount of transition metal source (calculated as transition metal element) is denoted as M3. The ratio of M1:M2:M3 is (2-4):1:(0.025-0.07).

[0024] (3) Mix the first suspension with the second suspension and then perform an aging treatment to obtain the catalyst precursor;

[0025] (4) The catalyst precursor is calcined.

[0026] In existing technologies, conventional catalyst preparation methods, such as impregnation or precipitation, result in catalysts with poor dispersion of active components, which is detrimental to the activity of these components. According to the preparation method of this invention, by strictly controlling the ratio of divalent metals (nickel and magnesium) to trivalent metals (aluminum and rare earth elements) in the chemical composition, and simultaneously strictly controlling the pH value of the solution during precipitation, the utilization efficiency of the catalyst preparation raw materials can be effectively improved. After aging treatment, a stable and crystalline precursor with a hydrotalcite structure is obtained, which can improve the dispersion and utilization efficiency of each component in the prepared catalyst, especially Ni, thereby enhancing the catalytic activity of the catalyst. Furthermore, the catalyst provided by this invention does not require the introduction of noble metal components, which helps reduce the preparation cost. Through the synergistic effect of Ni, Mg, Al, rare earth elements, and the transition metal Zr, the catalyst finally prepared by this invention for the dehydrogenation of organic liquid hydrogen storage materials can achieve both high catalytic activity and excellent thermal stability.

[0027] In this invention, the "first suspension" and "second suspension" refer to solutions containing suspended solids, and the pH of the "first suspension" and "second suspension" refers to the pH of the liquid phase. In this invention, the pH value is obtained by measuring with a pH meter.

[0028] According to the present invention, the pH of the first suspension is 5-8, for example, it can be a specific pH value such as 9, 9.5, 10, 10.5, 11, or any range between the two. Preferably, the pH of the first suspension is 6.5-7.5. In the present invention, the pH of the first suspension is adjusted by controlling the amount of precipitant used in step (1).

[0029] According to the present invention, the pH of the second suspension is 4-7, for example, it can be a specific pH value such as 8, 8.5, 9, 9.5, 10, or any range between the two. Preferably, the pH of the second suspension is 5-6. In the present invention, the pH of the second suspension is adjusted by controlling the amount of alkali used in step (2).

[0030] In this invention, controlling the pH of the first suspension and the second suspension within the above-mentioned preferred range is beneficial to improving the utilization efficiency of the raw materials for catalyst preparation and obtaining a precursor with a stable composition and complete crystallization and a hydrotalcite structure.

[0031] According to some preferred embodiments of the present invention, the pH of the first suspension is not lower than the pH of the second suspension; preferably, the pH of the second suspension is 1-2 lower than the pH of the first suspension. Using the above preferred embodiments is beneficial for obtaining structurally stable hydrotalcite precursors.

[0032] In this invention, the total molar amount of nickel source (calculated as Ni) and magnesium source (calculated as Mg) is denoted as M1, the total molar amount of aluminum source (calculated as Al) and rare earth source (calculated as rare earth element) is denoted as M2, and the molar amount of transition metal source (calculated as transition metal element) is denoted as M3. The ratio of M1:M2:M3 is (2-4):1:(0.025-0.07), preferably (2.5-3.5):1:(0.04-0.065). Controlling the proportions of divalent metals (nickel and magnesium), trivalent metals (aluminum and rare earth), and transition metals in the catalyst chemical composition within the above-mentioned preferred range is beneficial to the ultra-high dispersion and utilization efficiency of the active components in the catalyst finally obtained by this invention, further improving the activity of the catalyst.

[0033] In a further preferred embodiment, the molar ratio of nickel source (calculated as Ni) to magnesium source (calculated as Mg) is (0.1-0.5):1, for example, it can be a specific molar ratio or a range between the two such as 0.1:1, 0.2:1, 0.3:1, 0.4:1, 0.5:1, etc. Preferably, the molar ratio of nickel source (calculated as Ni) to magnesium source (calculated as Mg) is (0.2-0.4):1.

[0034] In a further preferred embodiment, the molar ratio of the rare earth source (calculated as rare earth element) to the aluminum source (calculated as Al) is (0.005-0.03):1, for example, it can be a specific molar ratio or a range between the two such as 0.005:1, 0.008:1, 0.01:1, 0.015:1, 0.02:1, etc. Preferably, the molar ratio of the rare earth source (calculated as rare earth element) to the aluminum source (calculated as Al) is (0.01-0.03):1.

[0035] The present invention has a wide range of rare earth elements to be selected from the rare earth source. Preferably, the rare earth elements in the rare earth source are selected from at least one of La, Ce and Nd.

[0036] This invention does not particularly limit the specific types of nickel, magnesium, aluminum, and rare earth sources; conventional metal-soluble compounds can be used, as long as the corresponding metal element is provided. For example, it can be at least one of metal nitrates, acetates, oxalates, chlorides, and carbonates. Preferably, the nickel source can be at least one of nickel nitrate, basic nickel carbonate, nickel acetate, and nickel oxalate. The aforementioned soluble compounds may also contain water of crystallization, as is well known to those skilled in the art.

[0037] In step (1), a precursor solution can be prepared first, and then a precipitant can be added; alternatively, the precursor solution and the precipitant solution can be prepared separately and then mixed. Preferably, the precipitant is provided by the precipitant solution. The present invention does not particularly limit the solvent in the precursor solution and the precipitant solution; preferably, the solvent is water.

[0038] According to some preferred embodiments of the present invention, in step (1), the precipitant comprises sodium hydroxide and sodium carbonate. Preferably, the molar ratio of sodium hydroxide to sodium carbonate is (3-4):1, more preferably (3-3.5):1. The present invention does not particularly limit the amount of the precipitant used, as long as the pH of the first suspension formed is within the above-mentioned range.

[0039] In this invention, the molar ratio of zirconium to chromium is 1:(0.2-0.5), preferably 1:(0.25-0.5, based on elemental composition. In the above-mentioned preferred case, the stability of the catalyst can be further improved through the synergistic effect of zirconium and chromium.

[0040] The present invention does not particularly limit the specific type of the transition metal source, but rather takes into account the ability to provide the corresponding metal element. Preferably, the zirconium source can be zirconium nitrate and / or zirconium oxynitrate, and the chromium source can be chromic anhydride.

[0041] According to some preferred embodiments of the present invention, in step (2), the alkali is selected from at least one of ammonia, sodium bicarbonate, sodium hydroxide, and ammonium carbonate. The present invention does not have any particular requirements regarding the type of solvent; preferably, the solvent is water.

[0042] In step (2), the transition metal source can be dissolved in a solvent and then an alkali can be added; alternatively, the transition metal source and the alkali can be dissolved separately in a solvent and then mixed. Preferably, the alkali is provided by an aqueous solution of an alkali. In this invention, the amount of alkali used is sufficient to meet the pH of the second suspension.

[0043] In this invention, the first coprecipitation reaction and the second coprecipitation reaction can be carried out at room temperature (25±5℃).

[0044] According to the present invention, there is no particular limitation on the contact order of the first suspension and the second suspension in step (3). Preferably, the first suspension and the second suspension are mixed by adding the second suspension to the first suspension. Adopting the above-mentioned preferred embodiment facilitates sufficient contact between the two, which is beneficial to further improving the dispersion and utilization rate of Ni in the obtained catalyst and enhancing the catalyst activity.

[0045] In this invention, a precursor with a hydrotalcite structure is formed through the aging treatment. Preferably, in step (3), the aging treatment conditions include: a temperature of 70-90℃, more preferably 80-85℃; and a time of 2-4 hours, more preferably 3-4 hours. Using the above-mentioned preferred embodiments is beneficial for obtaining a precursor with a stable composition and complete crystallization, possessing a hydrotalcite structure.

[0046] According to the present invention, the preparation method may further include: optionally performing solid-liquid separation, washing, and drying on the product obtained from the aging treatment to obtain the catalyst precursor. The present invention specifically limits the methods and conditions for the solid-liquid separation, washing, and drying, which can be carried out using methods conventional in the art. Preferably, the solid-liquid separation can be performed by filtration.

[0047] Preferably, the washing process includes washing the filter cake obtained by the transition with water until the pH of the washing water is neutral.

[0048] Preferably, the drying temperature is 100-130℃ and the time is 12-18h.

[0049] According to some preferred embodiments of the present invention, in step (4), the calcination is carried out in an oxygen-containing atmosphere, which may be provided by oxygen or a mixture of oxygen and an inert gas, preferably nitrogen and / or argon. The volume content of oxygen in the oxygen-containing atmosphere is 20-100%.

[0050] Preferably, the oxygen-containing atmosphere is provided by air.

[0051] According to some preferred embodiments of the present invention, the calcination temperature is 400-500℃, preferably 400-450℃, and the time is 2-6h, preferably 4-5h.

[0052] According to the present invention, the preparation method may further include optionally molding the calcined catalyst powder. The molding can be carried out using conventional methods in the art; preferably, the molding is tableting, which can be performed using a tablet press with a punch pressure of, for example, 70-120 kN and a tablet diameter of 3-5 mm.

[0053] Preferably, to improve the strength of the formed catalyst, a forming aid, such as graphite powder, can be added during the forming process. The mass ratio of the graphite powder to the catalyst powder is (0.01-0.02):1.

[0054] According to the present invention, the catalyst calcined in step (4) can be used directly as a fresh catalyst, or it can be used after a reduction treatment. The reduction treatment can be carried out during catalyst preparation or before the catalyst is used, and those skilled in the art can choose according to actual needs. The specific reduction treatment method will be described later.

[0055] A second aspect of the present invention provides a catalyst prepared by the above-described preparation method.

[0056] A third aspect of the present invention provides a method for catalytic dehydrogenation of an organic liquid hydrogen storage material, the method comprising: contacting the organic liquid hydrogen storage material with a dehydrogenation catalyst under dehydrogenation reaction conditions;

[0057] The dehydrogenation catalyst is the catalyst described in the second aspect.

[0058] The present invention has a wide range of choices for the organic liquid hydrogen storage material. Preferably, the organic liquid hydrogen storage material is selected from methylcyclohexane, hydrogenated naphthalene, hydrogenated carbazole and hydrogenated N-ethylcarbazole, etc. The hydrogenated naphthalene can be, for example, tetrahydronaphthalene, decahydronaphthalene, etc., the hydrogenated N-ethylcarbazole can be, for example, perhydroN-ethylcarbazole, and the hydrogenated carbazole can be, for example, perhydrocarbazole.

[0059] According to some preferred embodiments of the present invention, the dehydrogenation reaction conditions include: a reaction temperature of 210-450°C, a reaction pressure of 0-1 MPa, and a liquid hourly space velocity (LHSV) of 0.3-5000 h⁻¹ for the organic liquid hydrogen storage material. -1 In this invention, unless otherwise specified, all reaction pressures are gauge pressures.

[0060] According to some preferred embodiments of the present invention, when the organic liquid hydrogen storage material is methylcyclohexane, the dehydrogenation reaction conditions include: a reaction temperature of 350-500°C, preferably 400-480°C; a reaction pressure of 0-1 MPa, preferably 0-0.1 MPa; and a liquid hourly space velocity (LHSV) of 200-5000 h⁻¹ for the organic liquid hydrogen storage material. -1 .

[0061] According to some preferred embodiments of the present invention, when the organic liquid hydrogen storage material is tetrahydronaphthalene, decahydronaphthalene, perhydroN-ethylcarbazole, and perhydrocarbazole, the dehydrogenation reaction conditions include: a reaction temperature of 200-250°C, preferably 210-230°C; a reaction pressure of 0-1 MPa, preferably 0-0.1 MPa; and a liquid hourly space velocity (LISH) of 0.3-1 h⁻¹ for the organic liquid hydrogen storage material. -1 Preferably, it is 0.35-0.5h. -1 .

[0062] According to the present invention, preferably, the method further includes reducing the dehydrogenation catalyst prior to contact. The reduction treatment can be carried out in a manner conventional in the art, as long as it enables at least a portion of the Ni element to be reduced to elemental form.

[0063] Preferably, the reduction treatment is carried out in the presence of hydrogen, and the temperature of the reduction treatment is 400-500℃, preferably 450-500℃; the pressure is 0-1MPa, preferably 0-0.1MPa.

[0064] The present invention will be described in detail below through embodiments.

[0065] In the following examples, all raw materials used were commercially available.

[0066] Example 1

[0067] (1) Dissolve 12.05g of Mg(NO3)2·6H2O, 3.78g of Ni(NO3)2·6H2O, 7.39g of Al(NO3)3·9H2O, and 0.13g of Ce(NO3)3·6H2O in pure water and stir at room temperature until completely dissolved to obtain a mixed salt solution containing nickel, magnesium, aluminum, and rare earth elements, denoted as the first solution; dissolve 6.40g of NaOH and 5.30g of Na2CO3 in pure water to obtain a mixed solution of sodium hydroxide and sodium carbonate, denoted as the second solution; under continuous stirring, add the first solution and the second solution dropwise to the reactor in parallel, controlling the solution to be alkaline during the dropwise addition process to obtain a first suspension containing solid suspended matter, the pH value of which is 6.8-6.9.

[0068] (2) Dissolve 0.1848g of ZrO(NO3)2 and 0.0375g of chromic anhydride in pure water to prepare a mixed solution of zirconium oxynitrate and chromic anhydride, which is referred to as the third solution; co-precipitate the third solution with NaOH aqueous solution to prepare a second suspension containing solid suspended matter, and control the pH value of the second suspension at 5.2-5.3.

[0069] (3) The second suspension is directly added to the first suspension and stirred and mixed. Then, it is aged at 80°C for 3-4 hours and then filtered. The resulting filter cake is washed with water until neutral and then dried at 100-130°C for 12 hours to obtain a precursor with a hydrotalcite structure.

[0070] (4) After grinding the precursor with the hydrotalcite structure, it was calcined at 400°C in air for 4 hours. After natural cooling, a small amount of graphite powder was added (the mass ratio of graphite powder to precursor was 0.01:1). The catalyst was then pressed into a cylindrical catalyst of Ф5×(3-4)mm using a single-punch tablet press (produced by Sinopharm Longli) with a punch pressure of 110kN. This catalyst was designated as CAT-1.

[0071] Example 2

[0072] (1) Dissolve 12.05g of Mg(NO3)2·6H2O, 3.78g of Ni(NO3)2·6H2O, 7.35g of Al(NO3)3·9H2O, and 0.18g of Gd(NO3)3·6H2O in pure water and stir at room temperature until completely dissolved to obtain a mixed salt solution containing nickel, magnesium, aluminum, and rare earth elements, which is denoted as the first solution; dissolve 6.40g of NaOH and 5.30g of Na2CO3 in pure water to obtain a mixed solution of sodium hydroxide and sodium carbonate, which is denoted as the second solution; under continuous stirring, add the first solution and the second solution dropwise to the reactor in parallel, and control the solution to be alkaline during the dropwise addition process to obtain a first suspension containing solid suspended matter, and control the pH value of the first suspension to be 6.8-6.9.

[0073] (2) Dissolve 0.2081g of ZrO(NO3)2 and 0.0375g of chromic anhydride in pure water to prepare a mixed solution of zirconium oxynitrate and chromic anhydride, which is referred to as the third solution; co-precipitate the third solution with NaOH aqueous solution to prepare a second suspension containing solid suspended matter, and control the pH value of the second suspension at 5.5-5.6.

[0074] (3) The second suspension is directly added to the first suspension and stirred and mixed. Then, it is aged at 80°C for 3-4 hours and then filtered. The resulting filter cake is washed with water until neutral and then dried at 100-130°C for 12 hours to obtain a precursor with a hydrotalcite structure.

[0075] (4) After grinding the precursor with the hydrotalcite structure, it was calcined at 400°C in air for 4 hours. After natural cooling, a small amount of graphite powder was added (the mass ratio of graphite powder to precursor was 0.01:1). The catalyst was then pressed into a cylindrical form of Ф5×(3-4)mm using a single-punch tablet press (produced by Sinopharm Longli) with a punch pressure of 100kN. This catalyst was designated as CAT-2.

[0076] Example 3

[0077] (1) Dissolve 11.79g of Mg(NO3)2·6H2O, 4.07g of Ni(NO3)2·6H2O, 7.35g of Al(NO3)3·9H2O, and 0.18g of Gd(NO3)3·6H2O in pure water and stir at room temperature until completely dissolved to obtain a mixed salt solution containing nickel, magnesium, aluminum, and rare earth elements, which is denoted as the first solution; dissolve 6.40g of NaOH and 5.30g of Na2CO3 in pure water to obtain a mixed solution of sodium hydroxide and sodium carbonate, which is denoted as the second solution; under continuous stirring, add the first solution and the second solution dropwise to the reactor in parallel, and control the solution to be alkaline during the dropwise addition process to obtain a first suspension containing solid suspended matter, and control the pH value of the first suspension to be 7.1-7.2.

[0078] (2) Dissolve 0.2312g of ZrO(NO3)2 and 0.0250g of chromic anhydride in pure water to prepare a mixed solution of zirconium oxynitrate and chromic anhydride, which is referred to as the third solution; co-precipitate the third solution with NaOH aqueous solution to prepare a second suspension containing solid suspended matter, and control the pH value of the second suspension at 5.8-5.9.

[0079] (3) The second suspension is directly added to the first suspension and stirred and mixed. Then, it is aged at 90°C for 3-4 hours and then filtered. The resulting filter cake is washed with water until neutral and then dried at 100-130°C for 12 hours to obtain a precursor with a hydrotalcite structure.

[0080] (4) After grinding the precursor with the hydrotalcite structure, it was calcined at 400°C in air for 4 hours. After natural cooling, a small amount of graphite powder was added (the mass ratio of graphite powder to precursor was 0.01:1). The catalyst was pressed into a cylindrical form of Ф5×(3-4)mm using a single-punch tablet press (produced by Sinopharm Longli) with a punch pressure of 100kN. This catalyst was designated as CAT-3.

[0081] Example 4

[0082] The method is the same as in Example 1, except that the amount of Mg(NO3)2·6H2O is 12.05g, the amount of Ni(NO3)2·6H2O is 7.56g, the amount of Al(NO3)3·9H2O is 7.39g, and the amount of Ce(NO3)3·6H2O is 0.13g.

[0083] The resulting catalyst is designated CAT-4.

[0084] Example 5

[0085] The method is the same as in Example 1, except that the pH of the first suspension is controlled to be 5.3-5.4 and the pH of the second suspension is controlled to be 5.2-5.3 by the amount of precipitant added.

[0086] The resulting catalyst is designated CAT-5.

[0087] Example 6

[0088] The method is the same as in Example 1, except that in step (2), the third solution does not contain chromic anhydride and the amount of ZrO(NO3)2 used is 0.2717g.

[0089] The resulting catalyst was designated CAT-6.

[0090] Comparative Example 1

[0091] (1) Dissolve 12.05g of Mg(NO3)2·6H2O, 3.78g of Ni(NO3)2·6H2O, 7.39g of Al(NO3)3·9H2O, 0.13g of Ce(NO3)3·6H2O, 0.3435g of ZrO(NO3)2 and 0.0375g of chromic anhydride in pure water and stir at room temperature until completely dissolved, which is recorded as the first solution; dissolve 6.40g of NaOH and 5.30g of Na2CO3 in pure water to prepare a mixed solution of sodium hydroxide and sodium carbonate, which is recorded as the second solution; under continuous stirring, the first solution and the second solution are added dropwise to the reactor in parallel, and the solution is controlled to be alkaline during the dropwise addition process to obtain the first suspension containing solid suspended matter.

[0092] (2) The first suspension is aged at 80°C for 3-4 hours, then filtered. The resulting filter cake is washed with water until neutral, and then dried at 100-130°C for 12 hours to obtain the precursor.

[0093] (3) After grinding the precursor, it is calcined at 400°C in air for 4 hours. After natural cooling, a small amount of graphite powder is added (the mass ratio of graphite powder to precursor is 0.01:1). The catalyst is pressed into a cylindrical form of Ф5×(3-4)mm using a single-punch tablet press (produced by Sinopharm Longli) with a punch pressure of 110kN. This is denoted as DCAT-1.

[0094] Comparative Example 2

[0095] The method is the same as in Example 1, except that Ni(NO3)2·6H2O is not added to the first solution in step (1).

[0096] The resulting catalyst is designated as DCAT-2.

[0097] Comparative Example 3

[0098] The method is the same as in Example 1, except that Ce(NO3)3·6H2O is not added to the first solution in step (1).

[0099] The resulting catalyst is designated as DCAT-3.

[0100] Comparative Example 4

[0101] 14.86 g of nickel nitrate hexahydrate was dissolved in deionized water, and 20 g of commercial alumina support (purchased from Yantai Heng Hui Chemical Co., Ltd.) was added. The sample was placed in a rotary evaporator and immersed at room temperature for 2 h. It was then dried at 100-130℃ for 12 h and calcined at 400℃ in air for 4 h. After natural cooling, a small amount of graphite powder (the mass ratio of graphite powder to precursor was 0.01:1) was added. The sample was then pressed into cylindrical catalysts of Ф5×(3-4) mm using a single-punch tablet press (produced by Sinopharm Longli) with a punch pressure of 110 kN. This catalyst was designated as DCAT-4.

[0102] Test case

[0103] The catalysts prepared in the above examples and comparative examples were reduced under hydrogen conditions for 4 hours at atmospheric pressure and a reduction temperature of 500°C.

[0104] 3g of the reduced catalyst was loaded into a fixed-bed reactor for the dehydrogenation reaction of the organic liquid hydrogen storage material. The reaction conditions are shown in Table 1. For example, the composition of the reactants and products was analyzed by online chromatography, and the reaction results were tested at 12 and 72 hours after feeding, as shown in Table 1.

[0105] In Table 1, when the raw material is perhydro-N-ethylcarbazole, the selectivity refers to the selectivity of N-ethylcarbazole; when the raw material is methylcyclohexane, the selectivity refers to the selectivity of the target product toluene.

[0106] Table 1

[0107]

[0108]

[0109] As can be seen from the results in Table 1, the catalyst prepared by the method provided in this invention can achieve both high catalytic activity and excellent stability in the dehydrogenation reaction of organic liquid hydrogen storage materials. It can exhibit high conversion rate and selectivity under relatively mild reaction conditions and can be applied to the dehydrogenation reaction of different organic liquid hydrogen storage materials, showing broad application prospects.

[0110] The preferred embodiments of the present invention have been described in detail above; however, the present invention is not limited thereto. Within the scope of the inventive concept, various simple modifications can be made to the technical solutions of the present invention, including combinations of various technical features in any other suitable manner. These simple modifications and combinations should also be considered as the content disclosed in the present invention and are all within the protection scope of the present invention.

Claims

1. A method for catalytic dehydrogenation of organic liquid hydrogen storage materials, characterized in that, The method includes: contacting an organic liquid hydrogen storage material with a dehydrogenation catalyst under dehydrogenation reaction conditions; The preparation method of the dehydrogenation catalyst includes the following steps: (1) Under stirring conditions, a precursor solution containing nickel source, magnesium source, aluminum source and rare earth source is mixed with a precipitant to carry out a first coprecipitation reaction to obtain a first suspension; the pH of the first suspension is 5-8; (2) A second coprecipitation reaction is carried out by mixing a transition metal source, an alkali and a solvent to obtain a second suspension; the pH of the second suspension is 4-7; the transition metal in the transition metal source includes zirconium and optionally chromium; The total molar amount of nickel source (calculated as Ni) and magnesium source (calculated as Mg) is denoted as M1, the total molar amount of aluminum source (calculated as Al) and rare earth source (calculated as rare earth element) is denoted as M2, and the molar amount of transition metal source (calculated as transition metal element) is denoted as M3. The ratio of M1:M2:M3 is (2-4):1:(0.025-0.07). (3) Mix the first suspension with the second suspension and then perform an aging treatment to obtain the catalyst precursor; (4) The catalyst precursor is calcined; The organic liquid hydrogen storage material is selected from at least one of methylcyclohexane, tetrahydronaphthalene, decahydronaphthalene, perhydroN-ethylcarbazole, and perhydrocarbazole; The rare earth element in the rare earth source is selected from at least one of La, Ce, Gd and Nd.

2. The method according to claim 1, wherein, The pH of the second suspension is 1-2 lower than that of the first suspension.

3. The method according to claim 1, wherein, The total molar amount of nickel source (calculated as Ni) and magnesium source (calculated as Mg) is denoted as M1, the total molar amount of aluminum source (calculated as Al) and rare earth source (calculated as rare earth element) is denoted as M2, and the molar amount of transition metal source (calculated as transition metal element) is denoted as M3. The ratio of M1:M2:M3 is (2.5-3.5):1:(0.04-0.065).

4. The method according to claim 1, wherein, The molar ratio of nickel source (calculated as Ni) to magnesium source (calculated as Mg) is (0.1-0.5):1; The molar ratio of rare earth source (calculated as rare earth element) to aluminum source (calculated as Al) is (0.005-0.03):

1.

5. The method according to any one of claims 1-4, wherein, In step (1), the precipitant includes sodium hydroxide and sodium carbonate, wherein the molar ratio of sodium hydroxide to sodium carbonate is (3-4):

1.

6. The method according to any one of claims 1-4, wherein the molar ratio of zirconium to chromium is 1:(0.2-0.5).

7. The method according to any one of claims 1-4, wherein, In step (3), the aging treatment conditions include: a temperature of 70-90℃ and a time of 2-4h; In step (4), the calcination is carried out in an oxygen-containing atmosphere at a temperature of 400-500℃ for 2-6 hours.

8. The method according to any one of claims 1-4, wherein, The dehydrogenation reaction conditions include: reaction temperature is 200-500℃, reaction pressure is 0-1MPa, liquid hourly space velocity of the organic liquid hydrogen storage material is 0.3-5000h -1 .

9. The method according to claim 8, wherein, Prior to contact, the method further includes reducing the dehydrogenation catalyst; The reduction process is carried out in the presence of hydrogen gas at a temperature of 450-500℃, a pressure of 0-1MPa, and a reduction time of 4-5h.

Citation Information

Patent Citations

  • Fluidized bed catalyst for syngas methanation, preparation method thereof and applications thereof

    CN105381803A

  • Catalyst for catalyzing dehydrogenation of alcohols as well as preparation method and application of catalyst

    CN115106094A