A sagger suitable for medium pressure casting and preparation method thereof

By combining the formula of corundum, mullite and magnesia-aluminum spinel with specific particle sizes with epoxy resin and the medium-pressure casting process, the problem of mechanical strength and porosity of the sagger in ceramic firing is solved, saving resources and equipment investment. of reduction.

CN118439857BActive Publication Date: 2024-10-18TANGSHAN LONGCHANG PORCELAIN IND CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410903796.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-10-18
Estimated Expiration
2044-07-08

AI Technical Summary

Technical Problem

The existing saggers used in the ceramic firing process are difficult to achieve high mechanical strength and low porosity under medium-pressure casting, and the equipment investment is high, the area is large, and resources and energy are wasted seriously. High-pressure casting requires high hardware conditions and the effect is not good. good.

Method used

Use corundum, mullite and magnesia-aluminum spinel with specific particle sizes combined with bisphenol A-type epoxy resin to prepare the sagger through ball milling and medium-pressure casting processes. The particle size is controlled at 250-350 mesh, and epoxy resin and an appropriate amount are added. After water defoaming and medium pressure casting, it is then fired to 1200-1400°C.

Benefits of technology

The mechanical strength of the sagger is maintained under medium-pressure casting, the porosity is appropriate, and it is suitable for ceramic sintering applications, reducing equipment investment and resource consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the technical field of refractory sagger materials, and in particular to a sagger suitable for medium pressure casting and a preparation method thereof. The present invention adopts corundum, mullite and magnesium aluminum spinel of specific sizes, and combines with a binder epoxy resin, and finds that such a formula can withstand medium pressure casting without substantially losing mechanical strength, and the sagger also has an appropriate porosity, which is conducive to subsequent application in ceramic sintering.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of refractory sagger materials, and in particular to a sagger suitable for medium-pressure casting and a preparation method thereof. Background Art

[0002] The saggers used in the firing process of daily-use ceramics usually adopt the 350T-500T hydraulic forming process. This equipment has high investment, large floor space, and produces special-shaped saggers with high thickness and large mass. In production, it not only greatly increases the labor intensity but also causes a lot of waste of resources and energy. There are also reports on the use of pressure casting process to form saggers. However, high-pressure casting is usually used, which has high hardware requirements for process equipment and conditions. When the casting pressure is low, it usually leads to the formed saggers with low mechanical strength and too many pores, which cannot be used for ceramic firing.

[0003] A Chinese patent with authorization announcement number CN108083823B discloses a composite sagger, a preparation method and application thereof; specifically, the composite sagger includes a base material and a fabric, and the base material is mainly prepared from kaolin, sillimanite of a specific particle size, alumina of a specific particle size, corundum of a specific particle size, andalusite of a specific particle size and mullite of a specific particle size. The raw materials of the above base materials are abundant in source and low in price, so the cost of the above base materials is low.

[0004] The Chinese patent with authorization announcement number CN113548884B discloses a sagger containing cordierite and composite spinel mullite and a preparation method thereof; specifically disclosed: the raw materials of the sagger contain the following components in parts by weight: 25 parts of spinel, 15 parts of cordierite, 40 parts of composite spinel mullite, 6 parts of kaolin, 2 parts of fused 98 magnesium oxide, 12 parts of calcined alumina powder, 1 part of yellow dextrin, and 3.2 parts of water.

[0005] The Chinese patent with the authorization announcement number CN111056834B discloses a method for preparing a spinel-mullite ceramic sagger; specifically disclosed: the ceramic sagger matrix is ​​prepared from raw materials and a colloidal solution, the components of the raw materials include 40-50% fused magnesium aluminum spinel, 15-25% fused mullite, 15-20% alumina powder, 4-8% aluminum titanate fine powder, 5-10% zirconium oxide, 3-5% magnesia powder, and 3-5% clay fine powder by weight percentage; the colloidal solution is a gel, and the components of the gel include 10-14% acrylamide, 0.2-0.4% methylene bisacrylamide, 0.4-0.6% ammonium persulfate, 0.2-0.4% tetramethylethylenediamine, and the rest is water by weight percentage; the weight of the gel is 8-12% of the total amount of the raw materials; and the process is completed by slurry preparation, injection molding, demolding, drying and sintering steps. Summary of the invention

[0006] In order to solve the above problems, the present invention provides a sagger suitable for medium pressure casting, wherein the sagger comprises the following raw materials in parts by weight: 15-25 parts of 100-120 mesh corundum, 5-10 parts of kaolin, 10-15 parts of talc, 26-32 parts of 2-1 mm mullite, 18-26 parts of 40-50 mesh magnesium aluminum spinel, and 12-16 parts of epoxy resin.

[0007] Furthermore, the particle size of the kaolin and talc is 250-350 meshes.

[0008] Furthermore, the epoxy resin is bisphenol A type epoxy resin E-12.

[0009] The present invention also provides a method for preparing the sagger suitable for medium pressure casting as described herein, which comprises the following steps:

[0010] (1) Grind corundum, kaolin, talc, mullite and magnesium aluminum spinel respectively with a ball mill, wherein the corundum is sieved through a 100-120 mesh sieve after ball milling, the magnesium aluminum spinel is sieved through a 40-50 mesh sieve after ball milling, the mullite is ball milled to a particle size of 2-1 mm, and the other raw materials are sieved through a 250-350 mesh sieve after ball milling;

[0011] (2) Mixing the raw materials in a kneader according to the required weight proportions to obtain a mixed powder, and then adding the required weight proportions of epoxy resin and an appropriate amount of water to the mixed powder, and continuing to mix to obtain a mixed material;

[0012] (3) After degassing the mixture, pour it into a mold at medium pressure to form a sagger body. After the body is formed, demould it and dry it until the moisture content is less than 2-5%;

[0013] (4) The obtained green body is fired at 1200-1400°C.

[0014] Furthermore, the amount of water added in step (2) is such that the water content of the mixture is 18-25%.

[0015] Furthermore, the defoaming includes defoaming in a vacuum pulping mixer, and the vacuum degree is ≤0.095Mpa.

[0016] Furthermore, the medium pressure casting pressure is 0.5-1.5 MPa.

[0017] Furthermore, the firing time is 5-15h.

[0018] Beneficial effects of the present invention:

[0019] The present invention adopts corundum, mullite and magnesium aluminum spinel of specific sizes and combines them with a binder epoxy resin. It is found that such a formula can withstand medium-pressure casting without substantially losing mechanical strength. At the same time, the sagger also has an appropriate porosity, which is beneficial to subsequent application in ceramic sintering. DETAILED DESCRIPTION

[0020] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0021] Example 1

[0022] A sagger suitable for medium pressure casting, characterized in that the sagger comprises the following raw materials in parts by weight: 20 parts of 100-mesh corundum, 8 parts of kaolin, 13 parts of talc, 30 parts of 2-1 mm mullite, 22 parts of 40-mesh magnesium aluminum spinel, and 15 parts of bisphenol A epoxy resin E-12, and the preparation method thereof comprises the following steps:

[0023] Grind corundum, kaolin, talc, mullite and magnesium aluminum spinel with a ball mill respectively, wherein the corundum is sieved through a 100-mesh sieve after ball milling, the magnesium aluminum spinel is sieved through a 40-mesh sieve after ball milling, the mullite is ball milled to a particle size of 2-1 mm, and the other raw materials are sieved through a 300-mesh sieve after ball milling;

[0024] The raw materials are mixed in a kneader according to the required weight parts to obtain a mixed powder, and then the required weight parts of epoxy resin and an appropriate amount of water are added to the mixed powder, and the mixture is further mixed to obtain a mixture, so that the water content of the mixture is 25%;

[0025] The mixture is defoamed in a vacuum mixer (vacuum degree ≤ 0.095Mpa), poured into a mold at medium pressure to form a sagger body (pressure 0.8MPa), and after the body is formed, it is demoulded and dried until the moisture content is less than 2%;

[0026] The obtained green body is fired at 1400°C for 8h.

[0027] Example 2

[0028] A sagger suitable for medium pressure casting, characterized in that the sagger comprises the following raw materials in parts by weight: 20 parts of 120-mesh corundum, 8 parts of kaolin, 13 parts of talc, 30 parts of 2-1 mm mullite, 22 parts of 50-mesh magnesium aluminum spinel, and 15 parts of bisphenol A epoxy resin E-12, and the preparation method thereof comprises the following steps:

[0029] Grind corundum, kaolin, talc, mullite and magnesium aluminum spinel respectively with a ball mill, wherein the corundum is sieved through a 120-mesh sieve after ball milling, the magnesium aluminum spinel is sieved through a 50-mesh sieve after ball milling, the mullite is ball milled to a particle size of 2-1 mm, and the other raw materials are sieved through a 300-mesh sieve after ball milling;

[0030] The raw materials are mixed in a kneader according to the required weight parts to obtain a mixed powder, and then the required weight parts of epoxy resin and an appropriate amount of water are added to the mixed powder, and the mixture is further mixed to obtain a mixture, so that the water content of the mixture is 20%;

[0031] The mixture is defoamed in a vacuum mixer (vacuum degree ≤ 0.095Mpa), poured into a mold at medium pressure to form a sagger body (pressure 1.5MPa), and after the body is formed, it is demoulded and dried until the moisture content is less than 2%;

[0032] The obtained green body is fired at 1300°C for 10 hours.

[0033] Comparative Example 1

[0034] A sagger suitable for medium pressure casting, which differs from Example 1 in that the corundum, mullite and magnesium aluminum spinel used are all ball-milled to 300 meshes.

[0035] Comparative Example 2

[0036] A sagger suitable for medium-pressure casting, which differs from Comparative Example 1 in that an air compressor is used to pressurize the inside of the container to 2 MPa.

[0037] Comparative Example 3

[0038] A sagger suitable for medium-pressure casting, which differs from Comparative Example 1 in that an air compressor is used to pressurize the inside of the container to 5 MPa.

[0039] Comparative Example 4

[0040] A sagger suitable for medium pressure casting, which differs from Example 1 in that the magnesium aluminum spinel used is ball-milled to 60 mesh.

[0041] Comparative Example 5

[0042] A sagger suitable for medium pressure casting, which differs from Example 1 in that the magnesium aluminum spinel used is ball-milled to 100 mesh.

[0043] Comparative Example 6

[0044] A sagger suitable for medium pressure casting, which differs from Example 1 in that the corundum balls used are ground to 60 meshes.

[0045] Comparative Example 7

[0046] A sagger suitable for medium pressure casting, which differs from Example 1 in that the corundum balls used are ground to 200 meshes.

[0047] Comparative Example 8

[0048] A sagger suitable for medium pressure casting, which differs from Example 1 in that the mullite used is ball-milled to 50 meshes.

[0049] Comparative Example 9

[0050] A sagger suitable for medium pressure casting, which differs from Example 1 in that epoxy resin is not used.

[0051] Comparative Example 10

[0052] A sagger suitable for medium-pressure casting, which differs from Example 1 in that an air compressor is used to pressurize the inside of the container to 0.3 MPa.

[0053] The performances of the saggers of Example 1, Example 2 and Comparative Examples 1-9 were tested respectively, and the results are shown in Table 1.

[0054] Table 1 Product performance test results of the embodiments and comparative examples

[0055]

[0056] From the results of Comparative Examples 1-3 in Table 1, it can be seen that when the raw materials of the present invention are used but the particle size control is not performed, a sagger with good mechanical strength and porosity cannot be obtained under medium pressure casting, and the performance of the sagger can only be improved under high pressure casting. From the results of Comparative Examples 4-8, it can also be found that the specific particle size control adopted by the present invention is crucial for achieving a sagger with the best mechanical strength. When epoxy resin is not used, it can be seen that the sagger has significant differences in both mechanical strength and porosity compared with Example 1, indicating that the addition of epoxy resin is also indispensable for the sagger of the present invention. From Comparative Example 10, it can be seen that the raw materials of the present invention cannot obtain a sagger with higher performance when cast under relatively low pressure.

[0057] It should be noted that the preferred embodiments of the present invention are given in the specification of the present invention, but the present invention can be implemented in many different forms and is not limited to the embodiments described in this specification. These embodiments are not intended to be additional limitations on the content of the present invention. The purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive. In addition, the above-mentioned technical features continue to be combined with each other to form various embodiments not listed above, which are all considered to be within the scope of the present invention specification; further, for ordinary technicians in this field, they can be improved or transformed according to the above description, and all these improvements and transformations should belong to the protection scope of the claims attached to the present invention.

Claims

1. A sagger suitable for medium pressure casting, characterized in that: The sagger is composed of the following raw materials in parts by weight: 15-25 parts of 100-120 mesh corundum, 5-10 parts of kaolin, 10-15 parts of talc, 26-32 parts of 2-1 mm mullite, 18-26 parts of 40-50 mesh magnesium aluminum spinel, and 12-16 parts of epoxy resin; The sagger is prepared by medium-pressure casting under a pressure of 0.5-1.5 MPa.

2. The sagger suitable for medium pressure casting according to claim 1, characterized in that: The particle size of the kaolin and talc is 250-350 meshes.

3. The sagger suitable for medium pressure casting according to claim 1, characterized in that: The epoxy resin is bisphenol A type epoxy resin E-12.

4. The method for preparing a sagger suitable for medium pressure casting according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) Grind corundum, kaolin, talc, mullite and magnesium aluminum spinel respectively with a ball mill, wherein the corundum is sieved through a 100-120 mesh sieve after ball milling, the magnesium aluminum spinel is sieved through a 40-50 mesh sieve after ball milling, the mullite is ball milled to a particle size of 2-1 mm, and the other raw materials are sieved through a 250-350 mesh sieve after ball milling; (2) Mixing the raw materials in a kneader according to the required weight proportions to obtain a mixed powder, and then adding the required weight proportions of epoxy resin and an appropriate amount of water to the mixed powder, and continuing to mix to obtain a mixed material; (3) After degassing the mixture, pour it into a mold at medium pressure to form a sagger body. After the body is formed, demould it and dry it until the moisture content is less than 2-5%; (4) The obtained green body is fired at 1200-1400°C.

5. The preparation method according to claim 4, characterized in that: The amount of water added in step (2) is such that the water content of the mixture is 18-25%.

6. The preparation method according to claim 4, characterized in that: The defoaming process includes defoaming in a vacuum pulping mixer, and the vacuum degree is ≤0.095MPa.

7. The preparation method according to claim 4, characterized in that: The pressure of the medium pressure casting is 0.5-1.5 MPa.

8. The preparation method according to claim 4, characterized in that: The firing time is 5-15h.

Citation Information

Patent Citations

  • Composite saggers, their preparation methods and applications

    CN108083823B

  • A method for preparing a spinel-mullite ceramic sagger

    CN111056834B

  • Sagger containing cordierite and composite spinel mullite and its preparation method

    CN113548884B

  • Formula and production technology of specially-shaped sagger produced by medium-pressure pouring process

    CN106699126A

  • Preparation method of spinel-mullite ceramic sagger

    CN111056834A