A super-hydrophobic, highly oleophobic, impact-resistant coating and preparation method thereof

By constructing a superhydrophobic high oleophobic impact resistance coating under the synergistic action of hydrophobic porous cerium oxide and biocatalyst, the problem of poor impact resistance of existing hydrophobic oleophobic coating under harsh conditions is solved, and the coating is realized High performance and simplified preparation process improve the durability and application value of the coating.

CN118440575BActive Publication Date: 2024-12-06CCTEG CHINA COAL RES INST
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410460580.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-16
Publication Date
2024-12-06
Estimated Expiration
2044-04-16

AI Technical Summary

Technical Problem

The existing hydrophobic and oleophobic coatings have poor impact resistance under harsh reaction conditions, which is difficult to meet the requirements of chemical reactors, and the preparation process is complex, and the mechanical properties of nanoparticle coatings are poor, affecting durability.

Method used

The synergistic effect of coral-like hydrophobic porous cerium oxide and biocatalyst is adopted to build a superhydrophobic and high oleophobic impact resistance coating by optimizing the coating formulation and process, and improve the impact resistance and hydrophobic and oleophobic properties of the coating.

Benefits of technology

The coating is unified with high hydrophobic, high oleophobic and impact resistance, simplifies the preparation process, and improves the durability and application value of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118440575B_ABST
    Figure CN118440575B_ABST
Patent Text Reader

Abstract

The present invention proposes a kind of super-hydrophobic high oleophobic impact-resistant coating and preparation method thereof, and the coating includes two components of A and B;Wherein, component A includes the following components in mass fractions:45‑50 parts of ethyl acetate, 28‑32 parts of propylene glycol methyl ether acetate, 17‑20 parts of polyhydroxy acrylic resin, 3‑5 parts of hydroxy silicone oil, 1.5‑5 parts of polycaprolactone polyol, 0.1‑0.5 parts of silane coupling agent KH570, 0.005‑0.001 parts of coral-like hydrophobic porous cerium oxide;Component B includes the following components in mass fractions:30‑33 parts of HDI trimer, 40‑50 parts of butyl acetate, 3‑5 parts of S150 solvent oil, 16‑18 parts of propylene glycol methyl ether acetate, 0.005‑0.01 parts of biocatalyst. The present invention is composed by optimizing the formula of the coating so that the coating has both super-hydrophobicity, high oleophobicity and impact resistance, and has a wide range of application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of coatings, and in particular, relates to a super-hydrophobic, highly oleophobic, impact-resistant coating and a preparation method thereof. Background Art

[0002] Hydrophobic and oleophobic coatings have excellent waterproof and antifouling capabilities, corrosion resistance and easy-to-clean properties, which can enhance the durability and practicality of products. Therefore, they are widely used in many industries. For example, in the electrolysis of water to produce hydrogen, hydrophobic and oleophobic coatings can protect electrolytic cells from immersion corrosion by electrolytes; in the chemical industry, coating the inner wall of the reactor with hydrophobic and oleophobic coatings can reduce the deposition of adhesions, increase system fluidity, and improve the efficiency of wall flushing; in the shipbuilding field, hydrophobic and oleophobic coatings can be used to reduce the attachment of marine organisms, reduce navigation resistance, save fuel and extend the life of the hull; in the aerospace field, hydrophobic and oleophobic coatings can improve the anti-icing ability of the aircraft surface and ensure flight safety; the application of hydrophobic and oleophobic coatings to solar panels can reduce dust accumulation and improve photoelectric conversion The coating can effectively prevent corrosion and improve the durability and reliability of metal structures. Plastics and textiles can obtain better waterproof performance through the hydrophobic and oleophobic coating, which increases the practicality and comfort of the products. The service life and durability of leather and wood products will also be improved by the application of hydrophobic and oleophobic coatings. Personal protective equipment such as gloves and clothing provide better waterproof and antifouling protection after hydrophobic and oleophobic treatment. Building materials such as concrete countertops are easier to maintain and clean after using hydrophobic and oleophobic coatings. Fasteners are coated with hydrophobic and oleophobic coatings, and their corrosion resistance and durability will be enhanced, thereby ensuring the stable connection and safety of the structure. In short, the wide application of hydrophobic and oleophobic coatings has brought substantial improvements to various industries and is one of the key technologies for improving material performance and extending service life.

[0003] Although hydrophobic and oleophobic coatings bring many benefits, there are also some problems and challenges in practical applications. Among them, the poor impact resistance of hydrophobic and oleophobic coatings has become a problem that cannot be ignored, especially when it is used as a coating material for chemical reactors. Since these materials are often faced with harsh reaction conditions, hydrophobic and oleophobic coatings may be subjected to continuous impact and erosion from particulate matter and acid-base compounds from the reaction system. These influencing factors may cause wear, peeling or degradation of the coating, thereby reducing the waterproof and antifouling properties and overall protective effect of the coating, which not only affects the appearance and aesthetics, but may also have a negative impact on the maintenance cost and service life of the reactor. Summary of the invention

[0004] The present invention is based on the inventor's discovery and understanding of the following facts and problems: a hydrophobic and oleophobic coating refers to a coating whose surface has a static contact angle (SCA) greater than 90° to a liquid, and has played an increasingly important role in the fields of antifouling, anticorrosion, antibacterial and drag reduction. At present, super-hydrophobic and highly oleophobic impact resistance cannot be effectively unified, and most hydrophobic and oleophobic coatings are constructed using inorganic nanoparticles / organic polymer hybrid materials. The preparation process is not only complicated and cumbersome, and the conditions are harsh, but also the nanoparticle-type hydrophobic and oleophobic coatings have poor mechanical properties, which affects the durability of the double-repellent properties, and the impact resistance is poor, and it is difficult to meet the requirements of practical applications. Therefore, the present invention aims to adopt a simple and easy method, based on the characteristics of high porosity and high specific surface area of ​​hydrophobic porous cerium oxide particles, and using biocatalysts to accelerate the room temperature curing speed of the coating, effectively utilizing the synergistic effect of hydrophobic porous cerium oxide and biocatalysts, and constructing a durable hydrophobic and oleophobic coating.

[0005] To achieve the above-mentioned purpose, an embodiment of the present invention provides a super-hydrophobic and highly oleophobic impact-resistant coating, comprising a component A and a component B;

[0006] The component A comprises the following components in parts by mass: 45-50 parts of ethyl acetate, 28-32 parts of propylene glycol methyl ether acetate, 17-20 parts of polyhydroxy acrylic resin, 3-5 parts of hydroxy silicone oil, 1.5-5 parts of polycaprolactone polyol, 0.1-0.5 parts of silane coupling agent KH570, and 0.005-0.001 parts of coral-like hydrophobic porous cerium oxide;

[0007] The B component comprises the following components in parts by mass: 30-33 parts of HDI trimer, 40-50 parts of butyl acetate, 3-5 parts of S150 solvent oil, 16-18 parts of propylene glycol methyl ether acetate, and 0.005-0.01 parts of biocatalyst.

[0008] The embodiment of the present invention optimizes the formulation of the coating, especially by adding coral-like hydrophobic porous cerium oxide to the coating, which has high porosity and high specific surface area, can absorb and disperse external impact energy in its porous structure, and exhibits good buffering performance, thereby improving the impact resistance of the coating; and the embodiment of the present invention can accelerate the curing speed of the coating at room temperature by introducing a biocatalyst, thereby ensuring the use of the coating in various service environments; in addition, the synergistic effect of the coral-like hydrophobic porous cerium oxide and the biocatalyst increases the number of micro-nano structures on the surface of the coating, further improving the hydrophobic and oleophobic properties of the coating, so the coating in the embodiment of the present invention has super hydrophobicity, high oleophobicity and impact resistance, and has a high application value.

[0009] In some embodiments, the mass ratio of the A component to the B component is (4-5):1.

[0010] In some embodiments, the hydroxyl content of the hydroxy silicone oil is 6-8%;

[0011] And / or, the molecular weight of the polycaprolactone polyol is 400-830.

[0012] In some embodiments, the particle size of the coral-like hydrophobic porous cerium oxide is 10-15 nm.

[0013] In some embodiments, the coral-like hydrophobic porous cerium oxide is prepared by a method comprising the following steps:

[0014] S1, adding chitosan powder to citric acid solution, stirring and mixing to form chitosan sol;

[0015] S2, dissolving cerium nitrate in a mixed solution of ethanol and silane coupling agent KH570 to obtain a cerium nitrate solution; and then stirring and mixing the chitosan sol and the cerium nitrate solution to obtain a gel solution;

[0016] S3, drying the gel solution and then calcining it, and finally grinding it to obtain the coral-like hydrophobic porous cerium oxide.

[0017] Furthermore, in step S1, the mass concentration of the citric acid solution is 5-15%, the mass volume ratio of the chitosan powder to the citric acid solution is 1 g: (20-50) mL; the stirring and mixing temperature is room temperature, and the mixing time is 2-5 h;

[0018] And / or, in step S2, the molar volume ratio of the cerium nitrate to the ethanol and the silane coupling agent KH570 is 0.02 mol:10 mL:2 mL, the stirring and mixing temperature is 30-40° C., and the mixing time is 2-4 h;

[0019] And / or, in the step S3, the drying temperature is 50-80°C, and the drying time is 2-5h; the calcination temperature is 550-650°C, and the calcination time is 3-4h.

[0020] In some embodiments, the biocatalyst comprises at least one of Herceptin, insulin, and growth hormone.

[0021] On the other hand, the embodiment of the present invention also provides a method for preparing the above-mentioned super-hydrophobic and highly oleophobic impact-resistant coating, comprising the following steps:

[0022] (1) At room temperature, component A and component B are stirred and mixed in proportion to obtain a mixed solution;

[0023] (2) The mixed solution is sprayed on the surface of the substrate and cured at room temperature to obtain the super-hydrophobic and highly oleophobic impact-resistant coating.

[0024] The method for preparing the super-hydrophobic and highly oleophobic impact-resistant coating according to the embodiment of the present invention has a simple and easy process, the raw materials used are convenient and easily available, the process conditions are easy for industrial scale-up production, and has broad application prospects.

[0025] In some embodiments, the preparation method of component A includes the following steps: stirring and mixing ethyl acetate and polyhydroxy acrylic resin evenly, then slowly adding hydroxy silicone oil, polycaprolactone polyol, and propylene glycol methyl ether acetate and stirring and mixing, and finally adding a mixture of silane coupling agent KH570 and coral-like hydrophobic porous cerium oxide, stirring and mixing evenly, and filtering with a 200-mesh filter to obtain component A.

[0026] In some embodiments, the preparation method of component B comprises the following steps: after mixing butyl acetate and HDI trimer evenly, slowly adding a mixture of propylene glycol methyl ether acetate and a biocatalyst and stirring evenly, and finally adding S150 solvent oil, stirring and mixing evenly, and filtering with a 200-mesh filter to obtain component B.

[0027] In some embodiments, the matrix includes one of Q235, Q195, Q215, and Q275. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a SEM image of the coral-like hydrophobic porous cerium oxide prepared in Example 1 of the present invention.

[0029] Figure 2 This is a TEM image of the coral-like hydrophobic porous cerium oxide prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0030] Embodiments of the present invention are described in detail below. The embodiments are exemplary and intended to be used to explain the present invention, but should not be construed as limiting the present invention.

[0031] Where values ​​are described herein as a range, it should be understood that such disclosure includes disclosure of all possible sub-ranges within that range, as well as specific values ​​falling within that range, regardless of whether a specific value or a specific sub-range is explicitly stated.

[0032] Herein, the words "comprises" and "includes" and variations thereof mean that other elements or integers which are permitted but not specifically described may be included.

[0033] In this article, the term "and / or" is merely a term used to describe the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B may represent three situations: A exists alone, A and B exist at the same time, and B exists alone.

[0034] In one aspect, an embodiment of the present invention provides a super-hydrophobic and highly oleophobic impact-resistant coating, comprising a component A and a component B;

[0035] The component A comprises the following components in parts by mass: 45-50 parts of ethyl acetate, 28-32 parts of propylene glycol methyl ether acetate, 17-20 parts of polyhydroxy acrylic resin, 3-5 parts of hydroxy silicone oil, 1.5-5 parts of polycaprolactone polyol, 0.1-0.5 parts of silane coupling agent KH570, and 0.005-0.001 parts of coral-like hydrophobic porous cerium oxide;

[0036] The B component comprises the following components in parts by mass: 30-33 parts of HDI trimer, 40-50 parts of butyl acetate, 3-5 parts of S150 solvent oil, 16-18 parts of propylene glycol methyl ether acetate, and 0.005-0.01 parts of biocatalyst.

[0037] In some embodiments, the mass ratio of the component A to the component B is (4-5):1, non-limiting examples include: 4:1, 4.5:1, 4.8:1 or 5:1, etc. If the mass ratio of component A is too high, the curing speed of the mixture of A and B at room temperature will be slowed down, affecting the actual process requirements; but if the mass ratio of component A is too low, the curing speed will also be slowed down. Therefore, the present application controls the mass ratio of component A to component B to be (4-5):1.

[0038] In some embodiments, the hydroxyl content of the hydroxy silicone oil is 6-8%, non-limiting examples include: 6%, 7%, 7.5% or 8%; if the hydroxyl content is too high, the system will be unstable and stratification will occur; but if the hydroxyl content is too low, the hydrophobic and oleophobic properties of the coating will deteriorate. Therefore, it is advantageous for the present application to control the hydroxyl content to 6-8%;

[0039] And / or, the molecular weight of the polycaprolactone polyol is 400-830, non-limiting examples include 400, 500, 600 or 830.

[0040] In some embodiments, the particle size of the coral-like hydrophobic porous cerium oxide is 10-15 nm, non-limiting examples include 10 nm, 12 nm, 14 nm or 15 nm.

[0041] The coral-like hydrophobic porous cerium oxide is prepared by a method comprising the following steps:

[0042] S1, adding chitosan powder to citric acid solution, stirring and mixing to form chitosan sol;

[0043] S2, dissolving cerium nitrate in a mixed solution of ethanol and silane coupling agent KH570 to obtain a cerium nitrate solution; and then stirring and mixing the chitosan sol and the cerium nitrate solution to obtain a gel solution;

[0044] S3, drying the gel solution and then calcining it, and finally grinding it to obtain the coral-like hydrophobic porous cerium oxide.

[0045] Further, in step S1, the mass concentration of the citric acid solution is 5-15%, non-limiting examples include: 5%, 8%, 10%, 12% or 15%; the mass volume ratio of the chitosan powder to the citric acid solution is 1g: (20-50) mL, non-limiting examples include: 1g: 20mL, 1g: 25mL, 1g: 30mL, 1g: 40mL, 1g: 45mL or 1g: 50mL; the stirring and mixing temperature is room temperature, and the mixing time is 2-5h, non-limiting examples include: 2h, 3h, 3.5h, 4h or 5h;

[0046] And / or, in step S2, the molar volume ratio of the cerium nitrate to the ethanol and the silane coupling agent KH570 is 0.02 mol:10 mL:2 mL; the stirring and mixing temperature is 30-40° C., non-limiting examples include: 30° C., 35° C., 38° C. or 40° C.; the mixing time is 2-4 h, non-limiting examples include: 2 h, 3 h, 3.5 h or 4 h;

[0047] And / or, in step S3, the drying temperature is 50-80°C, non-limiting examples include: 50°C, 60°C, 65°C, 70°C, 75°C or 80°C, etc.; the drying time is 2-5h, non-limiting examples include: 2h, 3h, 3.5h, 4h or 5h, etc.; the calcination temperature is 550-650°C, non-limiting examples include: 550°C, 580°C, 600°C, 620°C or 650°C, etc.; the calcination time is 3-4h, non-limiting examples include: 3h, 3.5h or 4h, etc.

[0048] By introducing coral-like hydrophobic porous cerium oxide into the coating, which has high porosity and high specific surface area, it can absorb and disperse external impact energy in its porous structure, showing good buffering properties, thereby improving the impact resistance of the coating.

[0049] In some embodiments, the biocatalyst includes at least one of Herceptin, insulin, and growth hormone. By adding the biocatalyst to the coating, the curing speed of the coating at room temperature can be accelerated, thereby improving the convenience of the coating spraying process.

[0050] On the other hand, the embodiment of the present invention also provides a method for preparing the above-mentioned super-hydrophobic and highly oleophobic impact-resistant coating, comprising the following steps:

[0051] (1) At room temperature, component A and component B are stirred and mixed in proportion to obtain a mixed solution;

[0052] (2) The mixed solution is sprayed on the surface of the substrate and cured at room temperature to obtain the super-hydrophobic and highly oleophobic impact-resistant coating.

[0053] In some embodiments, the preparation method of component A includes the following steps: stirring and mixing ethyl acetate and polyhydroxy acrylic resin evenly, then slowly adding hydroxy silicone oil, polycaprolactone polyol, and propylene glycol methyl ether acetate and stirring and mixing, and finally adding a mixture of silane coupling agent KH570 and coral-like hydrophobic porous cerium oxide, stirring and mixing evenly, and filtering with a 200-mesh filter to obtain component A.

[0054] In some embodiments, the preparation method of component B comprises the following steps: after mixing butyl acetate and HDI trimer evenly, slowly adding a mixture of propylene glycol methyl ether acetate and a biocatalyst and stirring evenly, and finally adding S150 solvent oil, stirring and mixing evenly, and filtering with a 200-mesh filter to obtain component B.

[0055] In some embodiments, the substrate includes one of Q235, Q195, Q215, and Q275. It should be noted that before spraying the A and B mixed solutions onto the substrate surface, the substrate needs to be subjected to ultrasonic decontamination treatment to ensure that the substrate surface is clean.

[0056] The following are non-limiting examples and comparative examples of the present invention. It should be noted that the schemes of the comparative examples are not prior art and are only provided for comparison with the schemes of the embodiments and are not intended to limit the present invention. Unless otherwise specified, the various raw materials used in the embodiments and comparative examples are conventional commercial products or can be prepared by known methods.

[0057] Example 1

[0058] The super-hydrophobic and highly oleophobic impact-resistant coating of this embodiment comprises component A and component B in a mass ratio of 5:1;

[0059] Component A includes the following components in parts by mass: 50 parts of ethyl acetate, 32 parts of propylene glycol methyl ether acetate, 18 parts of polyhydroxy acrylic resin, 5 parts of hydroxy silicone oil (the hydroxy content of the hydroxy silicone oil is 6%), 3 parts of polycaprolactone polyol (its molecular weight is 400), 0.4 parts of silane coupling agent KH570, and 0.003 parts of coral-like hydrophobic porous cerium oxide;

[0060] Component B includes the following components in parts by mass: 32 parts of HDI trimer, 45 parts of butyl acetate, 5 parts of S150 solvent oil, 18 parts of propylene glycol methyl ether acetate, and 0.01 parts of insulin.

[0061] The coral-like hydrophobic porous cerium oxide in component A of this embodiment is prepared by a method comprising the following steps:

[0062] S1, 1 g of chitosan powder was added to 20 mL of 10 wt % citric acid solution and stirred for 3 h at room temperature using a hot plate magnetic stirrer to form a chitosan sol of a light yellow colloidal solution;

[0063] S2, dissolving 0.02 mol of cerium nitrate in a mixed solution of 10 mL of ethanol and 2 mL of a silane coupling agent KH570 to obtain a cerium nitrate solution; then stirring and mixing the chitosan sol and the cerium nitrate solution at 40° C. for 3 h using the same hot plate magnetic stirrer to produce a uniform gel-like solution;

[0064] S3, drying the gel solution in an electric forced air drying furnace at 65°C for 3 hours, and then calcining it in a muffle furnace at 600°C for 4 hours to obtain a porous and loose light yellow block, which can be ground to obtain coral-like hydrophobic porous cerium oxide.

[0065] Figure 1 This is a SEM picture of the coral-like hydrophobic porous cerium oxide prepared in this example. It can be seen from the picture that the cerium oxide is coral-like and has a porous structure.

[0066] Figure 2 This is a TEM image of the coral-like hydrophobic porous cerium oxide prepared in this embodiment. It can be seen from the image that the particle size of the cerium oxide is about 15 nm.

[0067] This embodiment also provides a method for preparing the above-mentioned super-hydrophobic and highly oleophobic impact-resistant coating, comprising the following steps:

[0068] (1) At room temperature, component A and component B are stirred and mixed uniformly to obtain a mixed solution;

[0069] (2) The mixed solution is sprayed onto the Q235 steel after ultrasonic decontamination treatment using a spray gun, and then the sprayed sample is dried at room temperature until the coating sprayed on the Q235 steel is completely cured, thereby obtaining a super-hydrophobic, highly oleophobic and impact-resistant coating.

[0070] Example 2

[0071] The super-hydrophobic and highly oleophobic impact-resistant coatings of this embodiment are substantially the same as those of embodiment 1, except that: in component A, the mass fraction of the coral-like hydrophobic porous cerium oxide is 0.005 parts.

[0072] Example 3

[0073] The super-hydrophobic and highly oleophobic impact-resistant coating of this embodiment is substantially the same as that of Embodiment 1, except that: in component A, the mass fraction of hydroxy silicone oil is 4 parts, and the mass fraction of coral-like hydrophobic porous cerium oxide is 0.005 parts.

[0074] Example 4

[0075] The super-hydrophobic and highly oleophobic impact-resistant coatings of this embodiment are substantially the same as those of embodiment 1, except that: in component B, the mass fraction of insulin is 0.008 parts.

[0076] Example 5

[0077] The super-hydrophobic and highly oleophobic impact-resistant coatings of this embodiment are substantially the same as those of embodiment 1, except that: in component B, the mass fraction of growth hormone is 0.01 parts.

[0078] Comparative Example 1

[0079] The super-hydrophobic and highly oleophobic impact-resistant coating of this comparative example is substantially the same as that of Example 1, except that component A does not contain coral-like hydrophobic porous cerium oxide.

[0080] Comparative Example 2

[0081] The super-hydrophobic and highly oleophobic impact-resistant coating of this comparative example is substantially the same as that of Example 1, except that component B does not contain a biocatalyst.

[0082] The coatings prepared in the above examples and comparative examples were tested for hydrophobicity, oleophobicity, impact resistance and room temperature curing speed, and the results are shown in Table 1;

[0083] The test method of hydrophobic and oleophobic properties is as follows: using a contact angle meter to measure the contact angle of a water droplet or hexadecane on each coating surface, and recording the data to evaluate the hydrophobic and oleophobic properties of the coating;

[0084] The impact resistance test is carried out in accordance with GB / T 1732-2020 "Determination of impact resistance of paint films";

[0085] The room temperature curing speed adopts the natural curing observation method, and the curing speed of the coating is judged by observing the viscosity of the coating surface: if the coating is cured for 60 minutes and has no astringency, the room temperature curing effect is considered to be level 1; if the coating is cured for 70 minutes and has no astringency, the room temperature curing effect is considered to be level 2; if the coating is cured for 80 minutes and has no astringency, the room temperature curing effect is considered to be level 3; and so on, the curing speed of each coating is obtained.

[0086] Table 1

[0087]

[0088] It can be seen from Table 1 that compared with the coatings prepared in Comparative Examples 1 and 2, the coatings prepared in Examples 1-5 of the present invention by adding coral-like hydrophobic porous cerium oxide and a biocatalyst have larger hydrophobic contact angles and oleophobic contact angles, indicating that they have better hydrophobicity and oleophobicity; at the same time, they also have better impact resistance; and the coatings prepared in the embodiments of the present invention have a faster curing speed at room temperature and higher production efficiency.

[0089] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0090] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.

Claims

1. A super hydrophobic and highly oleophobic impact-resistant coating, characterized in that: It includes component A and component B; The component A comprises the following components in parts by mass: 45-50 parts of ethyl acetate, 28-32 parts of propylene glycol methyl ether acetate, 17-20 parts of polyhydroxy acrylic resin, 3-5 parts of hydroxy silicone oil, 1.5-5 parts of polycaprolactone polyol, 0.1-0.5 parts of silane coupling agent KH570, and 0.005-0.001 parts of coral-like hydrophobic porous cerium oxide; The B component includes the following components in parts by mass: 30-33 parts of HDI trimer, 40-50 parts of butyl acetate, 3-5 parts of S150 solvent oil, 16-18 parts of propylene glycol methyl ether acetate, and 0.005-0.01 parts of a biocatalyst; wherein the biocatalyst includes at least one of Herceptin, insulin, and growth hormone.

2. The super-hydrophobic and highly oleophobic impact-resistant coating according to claim 1, characterized in that: The mass ratio of the A component to the B component is (4-5):

1.

3. The super-hydrophobic and highly oleophobic impact-resistant coating according to claim 1, characterized in that: The hydroxyl content of the hydroxy silicone oil is 6-8%; And / or, the molecular weight of the polycaprolactone polyol is 400-830.

4. The super-hydrophobic and highly oleophobic impact-resistant coating according to claim 1, characterized in that: The particle size of the coral-like hydrophobic porous cerium oxide is 10-15 nm.

5. The super-hydrophobic and highly oleophobic impact-resistant coating according to claim 1, characterized in that: The coral-like hydrophobic porous cerium oxide is prepared by a method comprising the following steps: S1, adding chitosan powder to citric acid solution, stirring and mixing to form chitosan sol; S2, dissolving cerium nitrate in a mixed solution of ethanol and silane coupling agent KH570 to obtain a cerium nitrate solution; and then stirring and mixing the chitosan sol and the cerium nitrate solution to obtain a gel solution; S3, drying the gel solution and then calcining it, and finally grinding it to obtain the coral-like hydrophobic porous cerium oxide.

6. The super-hydrophobic and highly oleophobic impact-resistant coating according to claim 5, characterized in that: In the step S1, the mass concentration of the citric acid solution is 5-15%, and the mass volume ratio of the chitosan powder to the citric acid solution is 1 g: (20-50) mL; the stirring and mixing temperature is room temperature, and the mixing time is 2-5 h; And / or, in step S2, the molar volume ratio of the cerium nitrate to the ethanol and the silane coupling agent KH570 is 0.02 mol:10 mL:2 mL, the stirring and mixing temperature is 30-40° C., and the mixing time is 2-4 h; And / or, in the step S3, the drying temperature is 50-80°C, and the drying time is 2-5h; the calcination temperature is 550-650°C, and the calcination time is 3-4h.

7. A method for preparing a super-hydrophobic and highly oleophobic impact-resistant coating according to any one of claims 1 to 6, characterized in that: The steps include: (1) At room temperature, stir and mix component A and component B in proportion to obtain a mixed solution; (2) The mixed liquid is sprayed on the surface of the substrate and cured at room temperature to obtain the super hydrophobic, highly oleophobic and impact-resistant coating.

8. The method for preparing a super-hydrophobic and highly oleophobic impact-resistant coating according to claim 7, characterized in that: The preparation method of component A comprises the following steps: after ethyl acetate and polyhydroxy acrylic resin are stirred and mixed evenly, hydroxy silicone oil, polycaprolactone polyol and propylene glycol methyl ether acetate are slowly added and stirred and mixed, and finally a mixture of silane coupling agent KH570 and coral-like hydrophobic porous cerium oxide is added, and after stirring and mixing evenly, the mixture is filtered using a 200-mesh filter to obtain component A.

9. The method for preparing a super-hydrophobic and highly oleophobic impact-resistant coating according to claim 7, characterized in that: The preparation method of the B component comprises the following steps: after butyl acetate and HDI trimer are uniformly mixed, a mixture of propylene glycol methyl ether acetate and a biocatalyst is slowly added and stirred uniformly, and finally S150 solvent oil is added, and after stirring and mixing uniformly, the mixture is filtered using a 200-mesh filter to obtain the B component.

Citation Information

Patent Citations

  • Coralline rare earth oxide and preparation method thereof

    CN116924448A

  • Coating composition for forming ultra water repellentcoating layer, preparation method thereof and caotingmethod using the same

    KR1020060011218A

  • Irreversible immobilization of enzymes into polyurethane coatings

    US20030129314A1