A butterfly optical cable and its production process

By using modified carbon nanofiber filler and titanium dioxide modification technology in optical cables, the problem of insufficient pull and scratch resistance of optical cables is solved, excellent mechanical properties and light resistance are achieved, and the service life of optical cables is extended.

CN118444446BActive Publication Date: 2024-10-11ZHEJIANG DONGTONG OPTICAL NETWORK & IOT TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410892933.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-10-11
Estimated Expiration
2044-07-04

AI Technical Summary

Technical Problem

Existing optical cables have deficiencies in pull and scratch resistance, making it difficult to meet high-demand data transmission needs.

Method used

Modified carbon nanofiber filler is used to enhance the mechanical strength and light resistance of carbon fiber through hydrothermal reaction and chemical modification treatment, and is evenly dispersed in the butterfly sheath, combined with polyethylene, polyamide and ethylene-vinyl acetate copolymer. Forming materials with excellent mechanical properties.

Benefits of technology

Significantly improves the mechanical strength, high temperature resistance, aging resistance and bending resistance of the optical cable, slows down the sliding phenomenon of carbon fiber, enhances the light resistance of the sheath, and decomposes pollutants through the photocatalyst of titanium dioxide, extending the service life of the optical cable .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118444446B_ABST
    Figure CN118444446B_ABST
Patent Text Reader

Abstract

The present invention provides a butterfly optical cable and a production process thereof, wherein the butterfly optical cable comprises a butterfly sheath (1), an optical fiber (2) and a reinforcing member (3), wherein the optical fiber (2) is located at the center of the butterfly sheath (1), and the reinforcing member (3) is located at the two wings of the butterfly sheath (1), and the material of the butterfly sheath (1) comprises the following components by mass: 60-70 parts of polyethylene, 30-40 parts of polyamide, 15-25 parts of ethylene-vinyl acetate copolymer, 2-5 parts of antioxidant, 2-4 parts of maleic anhydride grafted polyethylene, 10-15 parts of modified carbon nanofiber filler, and 1-2 parts of polymethylvinylsiloxane. The optical cable has excellent high temperature resistance, aging resistance, tensile resistance and bending resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of communication optical cable manufacturing, and specifically relates to a butterfly optical cable and a production process thereof. Background Art

[0002] The vigorous development of 5G communications and artificial intelligence has also driven the development of a large number of related industries. As people's requirements for information transmission become higher and higher, they also put forward higher requirements for data transmission. The current development trend of optical cables is large wire diameter, large number of cores and extrusion stability, but poor tensile and scratch resistance. Butterfly optical cable is a new type of user access optical cable. According to the application environment and laying conditions, the optical cable structure and various technical parameters are reasonably designed. It combines the characteristics of indoor soft optical cable and self-supporting optical cable. It is produced with special equipment and imported precision molds. It is the best alternative product for FTTX network solutions and plays a unique role in the establishment of smart buildings, digital communities, campus networks, local area networks and other networks. Summary of the invention

[0003] The present invention provides a butterfly optical cable and a production process thereof, wherein the butterfly optical cable comprises a butterfly sheath 1, an optical fiber 2 and a reinforcing member 3, wherein the optical fiber 2 is located at the center of the butterfly sheath 1, and the reinforcing member 3 is located at the two wings of the butterfly sheath 1. The material of the butterfly sheath 1 comprises the following components by mass: 60-70 parts of polyethylene, 30-40 parts of polyamide, 15-25 parts of ethylene-vinyl acetate copolymer, 2-5 parts of antioxidant, 2-4 parts of maleic anhydride grafted polyethylene, 10-15 parts of modified carbon nanofiber filler, and 1-2 parts of polymethylvinylsiloxane. The optical cable has excellent high temperature resistance, aging resistance, tensile resistance and bending resistance.

[0004] The specific plan is as follows:

[0005] A butterfly optical cable, comprising a butterfly sheath 1, an optical fiber 2 and a reinforcing member 3, wherein the optical fiber 2 is located at the center of the butterfly sheath 1, and the reinforcing member 3 is located at the two wings of the butterfly sheath 1. The material of the butterfly sheath 1 comprises the following components by mass: 60-70 parts of polyethylene, 30-40 parts of polyamide, 15-25 parts of ethylene-vinyl acetate copolymer, 2-5 parts of antioxidant, 2-4 parts of maleic anhydride grafted polyethylene, 10-15 parts of modified carbon nanofiber filler, and 1-2 parts of polymethylvinylsiloxane;

[0006] The modified carbon nanofiber filler is prepared by the following method:

[0007] A) adding carbon nanofibers to a nitric acid aqueous solution, performing a hydrothermal reaction, filtering, washing, and drying to obtain activated carbon nanofibers;

[0008] B) adding activated carbon nanofibers to an ethanol solution of butyl titanate, adding acetic acid, hydrothermally reacting, filtering, washing, drying, and heating and calcining;

[0009] C) Take the product of step B, add 1-butyl-3-methylimidazole bromide and polyethylene glycol into N,N-dimethylformamide solvent and mix evenly, add azobisisobutyronitrile and stannous isooctanoate, stir evenly, let stand, perform hydrothermal reaction, filter, wash and dry to obtain.

[0010] Furthermore, the material of the butterfly sheath 1 includes the following components by mass: 63-66 parts of polyethylene, 35-40 parts of polyamide, 15-20 parts of ethylene-vinyl acetate copolymer, 3-5 parts of antioxidant, 2-4 parts of maleic anhydride grafted polyethylene, 13-15 parts of modified carbon nanofiber filler, and 1-2 parts of polymethylvinylsiloxane.

[0011] Furthermore, the modified carbon nanofiber filler is prepared by the following method:

[0012] A) Add 10g of carbon nanofibers to 200ml of 2-3mol / L nitric acid aqueous solution, perform hydrothermal reaction at 70-80℃ for 6-10h, filter, wash and dry to obtain activated carbon nanofibers;

[0013] B) Add 10g of activated carbon nanofibers to 200ml of 2-4wt% butyl titanate ethanol solution, add 10g of acetic acid, hydrothermally react at 70-80℃ for 5-10h, filter, wash, dry, and heat to 650-700℃ and calcine for 3-5h;

[0014] C) Take 10g of the product of step B, add 5-10g of 1-butyl-3-methylimidazole bromide and 4-6g of polyethylene glycol into 100ml of N,N-dimethylformamide and mix evenly, add 1-2g of azobisisobutyronitrile and 1-2g of stannous isooctanoate, stir evenly and let stand for 10-60min, then hydrothermally react at 70-90℃ for 3-6h, filter, wash and dry to obtain the product.

[0015] Furthermore, the length of the carbon nanofibers is 40-60 microns.

[0016] Furthermore, the antioxidant is antioxidant 1010.

[0017] A method for preparing a butterfly optical cable comprises preparing a modified carbon nanofiber filler, then adding polyethylene, polyamide, ethylene-vinyl acetate copolymer, antioxidant, maleic anhydride grafted polyethylene, modified carbon nanofiber filler, and polymethylvinylsiloxane into a blender according to a predetermined mass ratio, mixing them evenly to obtain a blended material, and coating and extruding the blended material on the surface of an optical fiber 2 and a reinforcing member 3 through a screw extruder to obtain the butterfly optical cable.

[0018] The present invention has the following beneficial effects:

[0019] Compared with the prior art, the beneficial effects of the present invention are:

[0020] 1) The titanium dioxide particles on the surface of the carbon fiber form protrusions on the fiber surface, which can anchor the carbon fiber in the sheath and slow down the slippage of the carbon fiber in the sheath layer. The modified carbon fiber filler increases the mechanical strength of the sheath layer, and titanium dioxide can absorb ultraviolet rays and improve the light resistance of the sheath. At the same time, titanium dioxide, as a good photocatalyst material, can also decompose pollutants on the surface of the optical cable, reduce cable pollution, and increase the service life of the optical cable;

[0021] 2) In order to prevent titanium dioxide particles from falling off from the surface of carbon fibers, after the titanium dioxide particles are deposited, a coating layer is formed on the surface of the carbon fibers by using polyionic liquids 1-butyl-3-methylimidazole bromide and polyethylene glycol. The π-π interaction between the imidazole ring cation in the ionic liquid and the surface of the carbon fibers tightly binds to the surface of the carbon fibers, thereby solidifying the titanium dioxide on the surface of the carbon fibers. The coating layer has a cross-linked structure, which is firmly coated on the carbon surface and is not easy to fall off. The carbon nanofibers and titanium dioxide particles are fully coated by copolymerization and cross-linking of 1-butyl-3-methylimidazole bromide and polyethylene glycol, and the coating is relatively uniform. The imidazole group of the ionic liquid can improve the dispersion of the filler in the sheath, and the coating of polyethylene glycol can also improve the bending resistance of the sheath.

[0022] 3) Through the optimization selection of other components, it was determined that polyethylene, polyamide, and ethylene-vinyl acetate copolymer have very excellent mechanical properties under the joint action of maleic anhydride grafted polyethylene and polymethylvinylsiloxane. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 is a cross-sectional view of the optical cable of the present invention. DETAILED DESCRIPTION

[0024] The present invention is further described below in conjunction with specific embodiments. In each embodiment and comparative example, the diameter of the reinforcing member 3 is 0.5 mm, and the thickness of the sheath is 0.3 mm; however, the protection scope of the present invention is not limited to the following embodiments, and any non-essential adjustments and modifications made to the present invention based on the above invention content still fall within the protection scope of the present invention.

[0025] Example 1

[0026] 10g of carbon nanofibers with a diameter of 40 microns were added to 200ml of 2mol / L nitric acid aqueous solution, and after hydrothermal reaction at 70°C for 10h, filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers; 10g of activated carbon nanofibers were added to 200ml of 2wt% butyl titanate ethanol solution, 10g of acetic acid was added, hydrothermal reaction was carried out at 70°C for 5h, filtered, washed with deionized water, dried at 80°C, and placed in a tubular furnace and heated to 650°C for calcination for 3h; 10g of the product was taken, added with 5g of 1-butyl-3-methylimidazole bromide and 4g of polyethylene glycol to 100ml of N,N-dimethylformamide and mixed evenly, 1g of azobisisobutyronitrile and 1g of stannous isooctanoate were added, stirred evenly and allowed to stand for 10min, then hydrothermally reacted at 70°C for 6h, filtered, washed with deionized water, and dried at 80°C to obtain modified carbon nanofiber filler.

[0027] 60 parts of polyethylene, 30 parts of polyamide, 15 parts of ethylene-vinyl acetate copolymer, 2 parts of antioxidant 1010, 2 parts of maleic anhydride grafted polyethylene, 10 parts of modified carbon nanofiber filler and 1 part of polymethylvinylsiloxane are added into a blender, heated and mixed evenly, and after mixing, extruded, cooled and pelletized to obtain a blended material, and the blended material is coated and extruded on the surface of the optical fiber 2 and the reinforcing member 3 through a screw extruder, wherein the optical fiber 2 is at the center of the butterfly sheath 1, and the reinforcing member 3 is on both wings of the butterfly sheath 1, to obtain the butterfly optical cable.

[0028] Example 2

[0029] 10g of carbon nanofibers with a diameter of 40 microns were added to 200ml of 3mol / L nitric acid aqueous solution, and after hydrothermal reaction at 80°C for 6h, filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers; 10g of activated carbon nanofibers were added to 200ml of 4wt% butyl titanate ethanol solution, 10g of acetic acid was added, hydrothermal reaction was carried out at 80°C for 5h, filtered, washed with deionized water, dried at 80°C, and placed in a tubular furnace and heated to 700°C for calcination for 3h; 10g of the product was taken, and 10g of 1-butyl-3-methylimidazole bromide and 6g of polyethylene glycol were added to 100ml of N,N-dimethylformamide and mixed evenly, 2g of azobisisobutyronitrile and 2g of stannous isooctanoate were added, stirred evenly and allowed to stand for 60min, followed by hydrothermal reaction at 90°C for 3h, filtered, washed with deionized water, and dried at 80°C to obtain modified carbon nanofiber filler.

[0030] 70 parts of polyethylene, 40 parts of polyamide, 25 parts of ethylene-vinyl acetate copolymer, 5 parts of antioxidant 1010, 4 parts of maleic anhydride grafted polyethylene, 15 parts of modified carbon nanofiber filler and 2 parts of polymethylvinylsiloxane are added into a blender, heated and mixed evenly, and after mixing, extruded, cooled and pelletized to obtain a blended material, and the blended material is coated and extruded on the surface of the optical fiber 2 and the reinforcing member 3 through a screw extruder, wherein the optical fiber 2 is at the center of the butterfly sheath 1, and the reinforcing member 3 is on both wings of the butterfly sheath 1, to obtain the butterfly optical cable.

[0031] Example 3

[0032] 10g of carbon nanofibers with a diameter of 40 microns were added to 200ml of 2.5mol / L nitric acid aqueous solution, and after hydrothermal reaction at 75°C for 8h, filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers; 10g of activated carbon nanofibers were added to 200ml of 3wt% butyl titanate ethanol solution, 10g of acetic acid was added, hydrothermal reaction was carried out at 75°C for 6h, filtered, washed with deionized water, dried at 80°C, and placed in a tubular furnace and heated to 670°C for calcination for 4h; 10g of the product was taken, added with 8g of 1-butyl-3-methylimidazole bromide and 5g of polyethylene glycol to 100ml of N,N-dimethylformamide and mixed evenly, 1.5g of azobisisobutyronitrile and 1.5g of stannous isooctanoate were added, stirred evenly and allowed to stand for 30min, then hydrothermally reacted at 80°C for 4h, filtered, washed with deionized water, and dried at 80°C to obtain modified carbon nanofiber filler.

[0033] 65 parts of polyethylene, 35 parts of polyamide, 20 parts of ethylene-vinyl acetate copolymer, 3 parts of antioxidant 1010, 3 parts of maleic anhydride grafted polyethylene, 12 parts of modified carbon nanofiber filler and 1.5 parts of polymethylvinylsiloxane are added into a blender, heated and mixed evenly, and after mixing, extruded, cooled and pelletized to obtain a blended material, and the blended material is coated and extruded on the surface of the optical fiber 2 and the reinforcing member 3 through a screw extruder, wherein the optical fiber 2 is at the center of the butterfly sheath 1, and the reinforcing member 3 is on both wings of the butterfly sheath 1, to obtain the butterfly optical cable.

[0034] Example 4

[0035] 10g of carbon nanofibers with a diameter of 40 microns were added to 200ml of 2.5mol / L nitric acid aqueous solution, and after hydrothermal reaction at 75°C for 8h, filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers; 10g of activated carbon nanofibers were added to 200ml of 3wt% butyl titanate ethanol solution, 10g of acetic acid was added, hydrothermal reaction was carried out at 75°C for 6h, filtered, washed with deionized water, dried at 80°C, and placed in a tubular furnace and heated to 670°C for calcination for 4h; 10g of the product was taken, added with 8g of 1-butyl-3-methylimidazole bromide and 5g of polyethylene glycol to 100ml of N,N-dimethylformamide and mixed evenly, 1.5g of azobisisobutyronitrile and 1.5g of stannous isooctanoate were added, stirred evenly and allowed to stand for 30min, then hydrothermally reacted at 80°C for 4h, filtered, washed with deionized water, and dried at 80°C to obtain modified carbon nanofiber filler.

[0036] 63 parts of polyethylene, 35 parts of polyamide, 25 parts of ethylene-vinyl acetate copolymer, 2 parts of antioxidant 1010, 4 parts of maleic anhydride grafted polyethylene, 15 parts of modified carbon nanofiber filler and 2 parts of polymethylvinylsiloxane are added into a blender, heated and mixed evenly, and after mixing, extruded, cooled and pelletized to obtain a blended material, and the blended material is coated and extruded on the surface of the optical fiber 2 and the reinforcing member 3 through a screw extruder, wherein the optical fiber 2 is at the center of the butterfly sheath 1, and the reinforcing member 3 is on both wings of the butterfly sheath 1, to obtain the butterfly optical cable.

[0037] Example 5

[0038] 10g of carbon nanofibers with a diameter of 40 microns were added to 200ml of 2.5mol / L nitric acid aqueous solution, and after hydrothermal reaction at 75°C for 8h, filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers; 10g of activated carbon nanofibers were added to 200ml of 3wt% butyl titanate ethanol solution, 10g of acetic acid was added, hydrothermal reaction was carried out at 75°C for 6h, filtered, washed with deionized water, dried at 80°C, and placed in a tubular furnace and heated to 670°C for calcination for 4h; 10g of the product was taken, added with 8g of 1-butyl-3-methylimidazole bromide and 5g of polyethylene glycol to 100ml of N,N-dimethylformamide and mixed evenly, 1.5g of azobisisobutyronitrile and 1.5g of stannous isooctanoate were added, stirred evenly and allowed to stand for 30min, then hydrothermally reacted at 80°C for 4h, filtered, washed with deionized water, and dried at 80°C to obtain modified carbon nanofiber filler.

[0039] 66 parts of polyethylene, 30 parts of polyamide, 15 parts of ethylene-vinyl acetate copolymer, 3 parts of antioxidant 1010, 2 parts of maleic anhydride grafted polyethylene, 10 parts of modified carbon nanofiber filler and 2 parts of polymethylvinylsiloxane are added into a blender, heated and mixed evenly, and after mixing, extruded, cooled and pelletized to obtain a blended material, and the blended material is coated and extruded on the surface of the optical fiber 2 and the reinforcing member 3 through a screw extruder, wherein the optical fiber 2 is at the center of the butterfly sheath 1, and the reinforcing member 3 is on both wings of the butterfly sheath 1, to obtain the butterfly optical cable.

[0040] Comparative Example 1

[0041] 70 parts of polyethylene, 30 parts of polyamide, 15 parts of ethylene-vinyl acetate copolymer, 3 parts of antioxidant 1010, 2 parts of maleic anhydride grafted polyethylene, 10 parts of carbon nanofiber filler with a diameter of 40 microns, and 2 parts of polymethylvinylsiloxane are added into a blender, heated and mixed evenly, and after mixing, extruded, cooled, and pelletized to obtain a blended material, and the blended material is coated and extruded on the surface of the optical fiber 2 and the reinforcing member 3 through a screw extruder, wherein the optical fiber 2 is at the center of the butterfly sheath 1, and the reinforcing member 3 is on the two wings of the butterfly sheath 1, to obtain the butterfly optical cable.

[0042] Comparative Example 2

[0043] 10 g of carbon nanofibers with a diameter of 40 microns were added to 200 ml of a 2.5 mol / L nitric acid aqueous solution, and subjected to hydrothermal reaction at 75°C for 8 hours. The mixture was filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers. 10 g of activated carbon nanofibers were added to 200 ml of a 3 wt% ethanol solution of butyl titanate, 10 g of acetic acid was added, and subjected to hydrothermal reaction at 75°C for 6 hours. The mixture was filtered, washed with deionized water, and dried at 80°C. The mixture was placed in a tubular furnace and heated to 670°C and calcined for 4 hours to obtain modified carbon nanofiber filler.

[0044] 70 parts of polyethylene, 30 parts of polyamide, 15 parts of ethylene-vinyl acetate copolymer, 3 parts of antioxidant 1010, 2 parts of maleic anhydride grafted polyethylene, 10 parts of modified carbon nanofiber filler and 2 parts of polymethylvinylsiloxane are added into a blender, heated and mixed evenly, and after mixing, extruded, cooled and pelletized to obtain a blended material, and the blended material is coated and extruded on the surface of the optical fiber 2 and the reinforcing member 3 through a screw extruder, wherein the optical fiber 2 is at the center of the butterfly sheath 1, and the reinforcing member 3 is on both wings of the butterfly sheath 1, to obtain the butterfly optical cable.

[0045] Comparative Example 3

[0046] 10 g of carbon nanofibers with a diameter of 40 μm were added to 200 ml of a 2.5 mol / L nitric acid aqueous solution, subjected to hydrothermal reaction at 75°C for 8 h, filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers; 10 g of activated carbon nanofibers, 8 g of 1-butyl-3-methylimidazole bromide, and 5 g of polyethylene glycol were added to 100 ml of N,N-dimethylformamide and mixed evenly, 1.5 g of azobisisobutyronitrile and 1.5 g of stannous isooctanoate were added, stirred evenly and allowed to stand for 30 min, followed by hydrothermal reaction at 80°C for 4 h, filtered, washed with deionized water, and dried at 80°C to obtain modified carbon nanofiber filler.

[0047] 70 parts of polyethylene, 30 parts of polyamide, 15 parts of ethylene-vinyl acetate copolymer, 3 parts of antioxidant 1010, 2 parts of maleic anhydride grafted polyethylene, 10 parts of modified carbon nanofiber filler and 2 parts of polymethylvinylsiloxane are added into a blender, heated and mixed evenly, and after mixing, extruded, cooled and pelletized to obtain a blended material, and the blended material is coated and extruded on the surface of the optical fiber 2 and the reinforcing member 3 through a screw extruder, wherein the optical fiber 2 is at the center of the butterfly sheath 1, and the reinforcing member 3 is on both wings of the butterfly sheath 1, to obtain the butterfly optical cable.

[0048] Comparative Example 4

[0049] 10g of carbon nanofibers with a diameter of 40 microns were added to 200ml of 2.5mol / L nitric acid aqueous solution, and after hydrothermal reaction at 75°C for 8h, filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers; 10g of activated carbon nanofibers were added to 200ml of 3wt% butyl titanate ethanol solution, 10g of acetic acid was added, hydrothermal reaction was carried out at 75°C for 6h, filtered, washed with deionized water, dried at 80°C, and placed in a tubular furnace and heated to 670°C for calcination for 4h; 10g of the product was taken, added to 8g of 1-butyl-3-methylimidazole bromide in 100ml of N,N-dimethylformamide and mixed evenly, 1.5g of azobisisobutyronitrile and 1.5g of stannous isooctanoate were added, stirred evenly and allowed to stand for 30min, then hydrothermally reacted at 80°C for 4h, filtered, washed with deionized water, and dried at 80°C to obtain modified carbon nanofiber filler.

[0050] 70 parts of polyethylene, 30 parts of polyamide, 15 parts of ethylene-vinyl acetate copolymer, 3 parts of antioxidant 1010, 2 parts of maleic anhydride grafted polyethylene, 10 parts of modified carbon nanofiber filler and 2 parts of polymethylvinylsiloxane are added into a blender, heated and mixed evenly, and after mixing, extruded, cooled and pelletized to obtain a blended material, and the blended material is coated and extruded on the surface of the optical fiber 2 and the reinforcing member 3 through a screw extruder, wherein the optical fiber 2 is at the center of the butterfly sheath 1, and the reinforcing member 3 is on both wings of the butterfly sheath 1, to obtain the butterfly optical cable.

[0051] Comparative Example 5

[0052] 10g of carbon nanofibers with a diameter of 40 microns were added to 200ml of 2.5mol / L nitric acid aqueous solution, and after hydrothermal reaction at 75°C for 8h, filtered, washed with deionized water, and dried at 80°C to obtain activated carbon nanofibers; 10g of activated carbon nanofibers were added to 200ml of 3wt% butyl titanate ethanol solution, 10g of acetic acid was added, hydrothermal reaction was carried out at 75°C for 6h, filtered, washed with deionized water, dried at 80°C, and heated to 670°C in a tubular furnace and calcined for 4h; 10g of the product was taken, added with 5g of polyethylene glycol to 100ml of N,N-dimethylformamide and mixed evenly, 1.5g of azobisisobutyronitrile and 1.5g of stannous isooctanoate were added, stirred evenly and allowed to stand for 30min, followed by hydrothermal reaction at 80°C for 4h, filtered, washed with deionized water, and dried at 80°C to obtain modified carbon nanofiber filler.

[0053] 70 parts of polyethylene, 30 parts of polyamide, 15 parts of ethylene-vinyl acetate copolymer, 3 parts of antioxidant 1010, 2 parts of maleic anhydride grafted polyethylene, 10 parts of modified carbon nanofiber filler and 2 parts of polymethylvinylsiloxane are added into a blender, heated and mixed evenly, and after mixing, extruded, cooled and pelletized to obtain a blended material, and the blended material is coated and extruded on the surface of the optical fiber 2 and the reinforcing member 3 through a screw extruder, wherein the optical fiber 2 is at the center of the butterfly sheath 1, and the reinforcing member 3 is on both wings of the butterfly sheath 1, to obtain the butterfly optical cable.

[0054] Experiments and Data

[0055] According to the national standard GB / T2951, the tensile strength of the sheath material, the tensile strength after thermal aging at 100℃ for 200h, and the environmental stress cracking time are tested.

[0056] YD / T1997.1-2022 "Introduction Optical Fiber Cables for Communications Part 1: Butterfly Optical Cables" conducts performance testing on optical cables and obtains repeated bending: residual additional attenuation.

[0057] The results are shown in Table 1.

[0058] Table 1

[0059]

[0060] Tests and Results

[0061] As can be seen from Table 1, the mechanical strength and bending resistance of the fiber modified only by titanium dioxide, or the carbon fiber modified only by 1-butyl-3-methylimidazole bromide and polyethylene glycol in one or both of azobisisobutyronitrile and stannous isooctoate, are not ideal, which proves that titanium dioxide modification, ionic liquid 1-butyl-3-methylimidazole bromide and polyethylene glycol in azobisisobutyronitrile and stannous isooctoate work together to form a carbon fiber filler with an anchoring function, which can increase the mechanical strength of the sheath layer. The filler of the present invention can be evenly dispersed in the polymer, thereby improving the bending resistance of the sheath.

[0062] Although the content of the present invention has been described in detail through the above preferred embodiments, the above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A butterfly optical cable, comprising a butterfly sheath (1), an optical fiber (2) and a reinforcing member (3), wherein the optical fiber (2) is located at the center of the butterfly sheath (1), and the reinforcing member (3) is located at two wings of the butterfly sheath (1), characterized in that: The material of the butterfly sheath (1) comprises the following components by weight: 60-70 parts of polyethylene, 30-40 parts of polyamide, 15-25 parts of ethylene-vinyl acetate copolymer, 2-5 parts of antioxidant, 2-4 parts of maleic anhydride grafted polyethylene, 10-15 parts of modified carbon nanofiber filler, and 1-2 parts of polymethylvinylsiloxane; The modified carbon nanofiber filler is prepared by the following method: after titanium dioxide particles are deposited, a coating layer is formed on the surface of carbon fibers by using polyionic liquid 1-butyl-3-methylimidazole bromide and polyethylene glycol, and the imidazole ring cation in the ionic liquid is tightly combined with the carbon fiber surface by the π-π interaction with the carbon fiber surface, thereby solidifying titanium dioxide on the surface of the carbon fiber, and the coating layer is a cross-linked structure, and the carbon nanofibers and titanium dioxide particles are fully coated by copolymerization and cross-linking of 1-butyl-3-methylimidazole bromide and polyethylene glycol, which specifically includes the following steps: A) adding 10 g of carbon nanofibers into 200 ml of 2-3 mol / L nitric acid aqueous solution, hydrothermally reacting at 70-80° C. for 6-10 h, filtering, washing, and drying to obtain activated carbon nanofibers; B) adding 10g of activated carbon nanofibers to 200ml of ethanol solution of butyl titanate with a concentration of 2-4wt%, adding 10g of acetic acid, hydrothermally reacting at 70-80℃ for 5-10h, filtering, washing, drying, heating to 650-700℃ and calcining for 3-5h; C) Take 10g of the product of step B, add 5-10g of 1-butyl-3-methylimidazole bromide and 4-6g of polyethylene glycol into 100ml of N,N-dimethylformamide and mix evenly, add 1-2g of azobisisobutyronitrile and 1-2g of stannous isooctanoate, stir evenly and let stand for 10-60min, then hydrothermally react at 70-90℃ for 3-6h, filter, wash and dry to obtain the product.

2. A butterfly optical cable as claimed in claim 1, characterized in that: The material of the butterfly sheath (1) comprises the following components by mass: 63-66 parts of polyethylene, 35-40 parts of polyamide, 15-20 parts of ethylene-vinyl acetate copolymer, 3-5 parts of antioxidant, 2-4 parts of maleic anhydride grafted polyethylene, 13-15 parts of modified carbon nanofiber filler, and 1-2 parts of polymethylvinylsiloxane.

3. A butterfly optical cable as claimed in claim 1, characterized in that: The length of the carbon nanofibers is 40-60 microns.

4. A butterfly optical cable as claimed in claim 1, characterized in that: The antioxidant is antioxidant 1010.

5. A method for preparing a butterfly optical cable according to any one of claims 1 to 4, characterized in that: A modified carbon nanofiber filler is prepared, and then polyethylene, polyamide, ethylene-vinyl acetate copolymer, antioxidant, maleic anhydride grafted polyethylene, modified carbon nanofiber filler, and polymethylvinylsiloxane are added to a blender according to a predetermined mass ratio and mixed evenly to obtain a blended material. The blended material is coated and extruded on the surface of the optical fiber (2) and the reinforcing member (3) through a screw extruder to obtain the butterfly optical cable.