A method for preparing porous filter material using blast furnace slag and its application
By calcining sodium carbonate, phosphogypsum and blast furnace slag and combining it with silane coupling agents and other substances to prepare porous filter materials, it solves the problem of removing organic and inorganic pollutants in landfill leachate and achieves efficient mercury ion adsorption and purification effects. The process flow is simplified and the cost is reduced.
Patent Information
- Application Number
- CN202410918013.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-10
AI Technical Summary
Existing technology is difficult to effectively remove organic and inorganic pollutants in landfill leachate, especially mercury ions, and the resource utilization method of blast furnace slag is complex and costly.
By mixing sodium carbonate, phosphogypsum and blast furnace slag and then calcining them, combined with silane coupling agent, silicone acrylic emulsion and sodium lauryl sulfate and other substances, a porous filter material is formed. High-speed stirring and steam curing processes are used to prepare a filter material with high performance. Porous filter material with adsorption properties.
It achieves efficient adsorption of COD and mercury ions in landfill leachate, significantly improves the purification effect, simplifies the process and reduces production costs.
Smart Images

Figure CN118459151B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of general industrial solid waste resource utilization, and in particular relates to a method for preparing porous filter material by utilizing blast furnace slag and application thereof. Background Art
[0002] Blast furnace slag is the solid waste discharged from the blast furnace when the blast furnace is smelting pig iron. It is mainly composed of gangue, ash and oxides in additives. During the blast furnace smelting process, the iron oxides in the iron ore are reduced to iron metal, and a large amount of heat energy is generated at the same time. As the temperature rises, the oxides in the ore and fuel begin to melt and complex physical and chemical reactions occur. These reactions cause the oxides and impurities in the ore to be separated and form slag. The composition of slag is mainly determined by the composition of the original ore, the addition of blast furnace fuel and various reactions during the smelting process.
[0003] After proper treatment and extraction, the components in blast furnace slag can be used to produce building materials, cement, road foundation materials, etc. Through resource utilization, the consumption of raw materials can be reduced and the pressure on the exploitation of natural resources can be reduced. The resource utilization of blast furnace slag can not only reduce production costs and improve resource utilization, but also drive the development of related industries, promote employment and economic growth. After processing, blast furnace slag can form granular materials with a certain pore structure and specific surface area. These granular materials have good adsorption and filtration properties and can be used in the filtration and adsorption process in sewage treatment. Blast furnace slag contains a certain amount of oxides such as iron, calcium, and silicon. These components can react chemically with harmful substances in sewage to form precipitation or complexes, thereby purifying sewage. At present, some studies and practices have shown that sewage filter materials prepared from blast furnace slag have good application effects in sewage treatment. Through appropriate process treatment, blast furnace slag can be processed into porous ceramic filter materials or activated carbon filter materials to remove pollutants such as organic matter and heavy metal ions in sewage. The sewage filter material prepared by blast furnace slag can be used as a new type of sewage treatment material to broaden the source of sewage treatment materials. The production of blast furnace slag is an inevitable process, but its value can be maximized through resource utilization. Therefore, the use of blast furnace slag to prepare sewage filter material is not only theoretically feasible, but also has important practical significance. Summary of the invention
[0004] Purpose of the invention: The purpose of the present invention is to provide a method for preparing a porous filter material using blast furnace slag. The prepared porous filter material can purify landfill leachate or sewage containing mercury ions.
[0005] Technical solution: The present invention provides a method for preparing a porous filter material using blast furnace slag, comprising the following steps:
[0006] (1) mixing sodium carbonate, phosphogypsum and blast furnace slag, grinding them into powder, and obtaining a carbon-phosphorus ash-slag mixed powder; calcining the carbon-phosphorus ash-slag mixed powder to obtain a calcined mixed powder;
[0007] (2) Mixing the silane coupling agent and the silicone-acrylic emulsion, stirring evenly, and obtaining a reinforced emulsion;
[0008] (3) mixing the polyester fiber powder and the calcined mixed powder prepared in step (1), stirring evenly to obtain fiber-mixed powder;
[0009] (4) mixing sodium lauryl sulfate, the strengthening emulsion prepared in step (2) and the fiber powder prepared in step (3), adding water to the mixture, and stirring at high speed to obtain a foaming slurry;
[0010] (5) pouring the foaming slurry prepared in step (4) into a mold for molding, and steam curing to obtain a porous filter material.
[0011] Furthermore, in step (1), the mass ratio of sodium carbonate, phosphogypsum and blast furnace slag is 5-25:25-75:100; the calcination temperature is 850-1150° C., and the calcination time is 1.5-4.5 hours.
[0012] Furthermore, the silane coupling agent in step (2) is KH-590.
[0013] Furthermore, the mass ratio of the silane coupling agent to the silicone-acrylic emulsion in step (2) is 5-25:100.
[0014] Furthermore, the mass ratio of the polyester fiber powder to the calcined mixed powder in step (3) is 0.5-2.5:100.
[0015] Furthermore, the mass ratio of sodium dodecyl sulfate, reinforcing emulsion and fiber powder in step (4) is 1.5~5.5:5~15:100; the liquid-solid ratio of water and mixed material is 0.25~0.45:1 mL / g; the stirring rate is 360~1440 rpm, and the stirring time is 2.5~12.5 minutes.
[0016] Furthermore, the steam curing temperature in step (5) is 180-360° C., and the curing time is 2-6 hours.
[0017] The invention also provides a porous filter material prepared according to the method.
[0018] The invention also provides application of the porous filter material in purifying garbage leachate or sewage.
[0019] Furthermore, the sewage contains mercury ions.
[0020] Reaction mechanism: Calcine the carbon-phosphorus ash slag mixed powder. Under high-temperature calcination, sodium carbonate and phosphogypsum react fully with silicates, iron oxides, and magnesium oxides in blast furnace slag, releasing carbon dioxide gas and water vapor to form an active mixture of sodium alkali-fused iron-magnesium doped with calcium silicate, calcium phosphate, and calcium sulfate. Mix the silane coupling agent KH-590 and silicone-acrylic emulsion. During the stirring process, the mercapto group in KH-590 reacts with the acrylic monomer in the silicone-acrylic emulsion to form a mercapto-loaded copolymer. Mix sodium dodecyl sulfate, reinforcing emulsion, and fiber powder, add water, and sodium dodecyl sulfate forms micelles in water and forms an adsorption film on the gas-liquid interface, thereby reducing the surface tension. Under high-speed stirring conditions, stable foam can be quickly formed, thereby causing the slurry to foam. The fiber powder undergoes a hydration reaction after contacting water to form a silicate gel mixed with calcium ferrosulfate and calcium iron phosphate-based materials. The hydrophilic groups of sodium dodecyl sulfate react with the active mineral components in the fiber powder, digesting and precipitating free calcium and magnesium oxides, and then mixing them into the silicate gel. The mercapto-loaded copolymers and acrylic monomers in the reinforced emulsion can react with iron, magnesium, and calcium cations to form an organic silicon complex mixture, which is then mixed into the silicate gel. During the steam curing process, the hydrophobic groups of sodium dodecyl sulfate can further react with acrylic monomers to induce the formation of copolymers, which encapsulate the hardened silicate hydration products.
[0021] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages: the present invention has a simple preparation process, makes full use of the blast furnace slag components, and realizes full resource utilization of blast furnace slag through simple processes such as mixing, stirring, and curing to prepare porous filter materials. The porous filter materials can effectively remove organic and inorganic pollutants in landfill leachate. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The figure is a flow chart of the processing method of the present invention. DETAILED DESCRIPTION
[0023] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.
[0024] Sampling and basic properties of domestic garbage leachate: The experimental garbage leachate was taken from Changshu No. 2 Waste Incineration Power Plant. The COD mass concentration of this batch of urban domestic garbage leachate was 4352 mg / L. Soluble mercury was added to the garbage leachate to make the mercury concentration reach 200 mg / L.
[0025] Blast furnace slag: Blast furnace slag comes from Leiyun Mineral Products Processing Plant in Lingshou County, mainly including 41.19% CaO, 38.26% SiO 2 、8.94%Al 2 O 3 、5.06%MgO、3.21%TiO 2、2.15%SO 3 and other components (loss on ignition and other inevitable impurities).
[0026] Example 1 Effect of the mass ratio of sodium carbonate, phosphogypsum and blast furnace slag on the performance of the prepared porous filter material water purifier
[0027] Sodium carbonate, phosphogypsum and blast furnace slag are mixed in a mass ratio of 2.5:25:100, 3:25:100, 4:25:100, 5:17.5:100, 5:20:100, 5:22.5:100, 5:25:100, 15:25:100, 25:25:100, 5:50:100, 15:50:100, 25:50:100, 5:75:100, 15:75:100, 25:75:100, 25:80:100, 25:85:100, 25:90:100, 27.5:75:100, 30:75:100, and 32.5:75:100, mixed, and ground into powder to obtain carbonphosphorus ash slag mixed powder. The carbon phosphorus ash mixed powder is calcined to obtain a calcined mixed powder, wherein the calcination temperature is 850°C and the calcination time is 1.5 hours. Silane coupling agent KH-590 and silicone acrylic emulsion are mixed in a mass ratio of 5:100, stirred evenly, and a reinforced emulsion is obtained. Polyester fiber powder and calcined mixed powder are mixed in a mass ratio of 0.5:100, stirred evenly, and fiber powder is obtained. Sodium dodecyl sulfate, reinforced emulsion and fiber powder are mixed in a mass ratio of 1.5:5:100, and then water is added to the mixture at a liquid-solid ratio of 0.25:1mL / g, followed by high-speed stirring to obtain a foaming slurry, which is poured into a mold for molding, steam-cured, and a porous filter material is obtained, wherein the stirring rate is 360rpm, the stirring time is 2.5 minutes, the steam curing temperature is 180°C, and the curing time is 2 hours.
[0028] Landfill leachate purification test: Weigh 1g of porous filter material and add it to 1L of landfill leachate, stir continuously for 30 minutes, centrifuge, and the supernatant obtained is the purified liquid after treatment.
[0029] COD concentration detection and calculation of COD adsorption capacity: The COD concentration of the leachate was determined in accordance with the national standard "Determination of Chemical Oxygen Demand of Water Quality - Dichromate Method" (HJ 828-2017). The COD adsorption capacity was calculated according to formula (1), where is the COD adsorption capacity (mg / g), and are the COD concentrations of domestic waste leachate before and after treatment (mg / L), V is the volume of leachate (1L), m is the mass of porous filter material (1g).
[0030] (1)
[0031] Mercury ion concentration detection and adsorption capacity calculation: The mercury ion concentration in the leachate was determined according to the "Determination of Mercury, Arsenic, Selenium, Bismuth and Antimony in Water by Atomic Fluorescence Method" (HJ 694-2014). The mercury ion adsorption capacity was calculated according to formula (2), where is the mercury ion adsorption capacity (mg / g), is the initial concentration of mercury ions in the leachate before treatment (mg / L), is the mercury ion concentration in the treated leachate (mg / L), V is the volume of the leachate (1L), m is the mass of porous filter material (1g).
[0032] (2)
[0033] The results of COD and mercury ion adsorption capacity are shown in Table 1.
[0034] Table 1 Effect of mass ratio of sodium carbonate, phosphogypsum and blast furnace slag on the performance of prepared porous filter media water purifier
[0035]
[0036] It can be seen from Table 1 that when the mass ratio of sodium carbonate, phosphogypsum and blast furnace slag is less than 5:25:100 (such as in Table 1, the mass ratio of sodium carbonate, phosphogypsum and blast furnace slag = 4:25:100, 3:25:100, 2.5:25:100, 5:22.5:100, 5:20:100, 5:17.5:100 and lower ratios not listed in Table 1), less sodium carbonate and phosphogypsum are added, and the materials react insufficiently during the calcination process, resulting in the COD and mercury ion adsorption capacity of the prepared porous filter material being significantly reduced as the mass ratio of sodium carbonate, phosphogypsum and blast furnace slag decreases. When the mass ratio of sodium carbonate, phosphogypsum and blast furnace slag is equal to 5~25:25~75:100 (as in Table 1, the mass ratio of sodium carbonate, phosphogypsum and blast furnace slag is 5:25:100, 15:25:100, 25:25:100, 5:50:100, 15:50:100, 25:50:100, 5:75:100, 15:75:100, 25:75:100), the carbon phosphate ash slag mixed powder is calcined, and sodium carbonate and phosphogypsum react fully with silicates, iron oxides and magnesium oxides in blast furnace slag under high temperature calcination environment, releasing carbon dioxide gas and water vapor to generate sodium alkali fused iron magnesium mixed with calcium silicate salt, calcium phosphate and calcium sulfate. Active mixture. Finally, the COD adsorption capacity of the prepared porous filter material water purifier is greater than 1322mg / g, and the mercury ion adsorption capacity is greater than 86mg / g. When the mass ratio of sodium carbonate, phosphogypsum and blast furnace slag is greater than 25:75:100 (such as in Table 1, the mass ratio of sodium carbonate, phosphogypsum and blast furnace slag = 25:80:100, 25:85:100, 25:90:100, 27.5:75:100, 30:75:100, 32.5:75:100 and higher ratios not listed in Table 1), excessive addition of sodium carbonate and phosphogypsum increases the impurity content during the calcination process, and reduces the production of silicate-based active materials, resulting in the COD and mercury ion adsorption capacity of the prepared porous filter material being significantly reduced as the mass ratio of sodium carbonate, phosphogypsum and blast furnace slag further increases. Therefore, in general, combining benefits and costs, when the mass ratio of sodium carbonate, phosphogypsum and blast furnace slag is equal to 5~25:25~75:100, it is most conducive to improving the adsorption performance of the prepared porous filter material.
[0037] Example 2 Effect of the mass ratio of silane coupling agent KH-590 and silicone-acrylic emulsion on the performance of the prepared porous filter material water purifier
[0038] Sodium carbonate, phosphogypsum and blast furnace slag are mixed in a mass ratio of 25:75:100, mixed and ground into powder to obtain carbon phosphorus ash slag mixed powder. The carbon phosphorus ash slag mixed powder is calcined to obtain a calcined mixed powder, wherein the calcination temperature is 1000°C and the calcination time is 3 hours. Silane coupling agent KH-590 and silicone acrylic emulsion are mixed in a mass ratio of 2.5:100, 3:100, 4:100, 5:100, 15:100, 25:100, 27.5:100, 30:100, 32.5:100, stirred evenly to obtain a reinforced emulsion. Polyester fiber powder and calcined mixed powder are mixed in a mass ratio of 1.5:100, stirred evenly to obtain fiber mixed powder. Sodium lauryl sulfate, reinforcing emulsion and fiber powder are mixed in a mass ratio of 3.5:10:100, and then water is added to the mixture in a liquid-to-solid ratio of 0.35:1 mL / g, followed by high-speed stirring to obtain a foaming slurry, which is poured into a mold for molding and steam-cured to obtain a porous filter material, wherein the stirring rate is 900 rpm, the stirring time is 7.5 minutes, the steam curing temperature is 270°C, and the curing time is 4 hours.
[0039] The landfill leachate purification test, COD concentration detection and COD adsorption capacity calculation, mercury ion concentration detection and adsorption capacity calculation are all the same as in Example 1. The COD and mercury ion adsorption capacity results are shown in Table 2.
[0040] Table 2 Effect of the mass ratio of silane coupling agent KH-590 and silicone-acrylic emulsion on the performance of the prepared porous filter media water purifier
[0041]
[0042] It can be seen from Table 2 that when the mass ratio of silane coupling agent KH-590 to silicone-acrylic emulsion is less than 5:100 (such as in Table 2, the mass ratio of silane coupling agent KH-590 to silicone-acrylic emulsion = 4:100, 3:100, 2.5:100 and lower ratios not listed in Table 2), less silane coupling agent KH-590 is added, and the reaction of silane coupling agent KH-590 and silicone-acrylic emulsion is insufficient, resulting in the COD and mercury ion adsorption capacity of the prepared porous filter material being significantly reduced as the mass ratio of silane coupling agent KH-590 to silicone-acrylic emulsion decreases. When the mass ratio of silane coupling agent KH-590 to silicone-acrylic emulsion is equal to 5-25:100 (as shown in Table 2, the mass ratio of silane coupling agent KH-590 to silicone-acrylic emulsion = 5:100, 15:100, 25:100), the silane coupling agent KH-590 and silicone-acrylic emulsion are mixed, and during the stirring process, the mercapto group in KH590 reacts with the acrylic monomer in the silicone-acrylic emulsion to form a mercapto-loaded copolymer. Finally, the COD adsorption capacity of the prepared porous filter material is greater than 1412 mg / g, and the mercury ion adsorption capacity is greater than 91 mg / g. When the mass ratio of silane coupling agent KH-590 to silicone-acrylic emulsion is greater than 25:100 (such as in Table 2, the mass ratio of silane coupling agent KH-590 to silicone-acrylic emulsion = 27.5:100, 30:100, 32.5:100 and higher ratios not listed in Table 2), the silane coupling agent KH-590 is added excessively, and the polymer generation is inhibited, resulting in the COD and mercury ion adsorption capacity of the prepared porous filter material being significantly reduced as the mass ratio of silane coupling agent KH-590 to silicone-acrylic emulsion further increases. Therefore, in general, combining benefits and costs, when the mass ratio of silane coupling agent KH-590 to silicone-acrylic emulsion is equal to 5~25:100, it is most conducive to improving the adsorption performance of the prepared porous filter material.
[0043] Example 3 Effect of the mass ratio of sodium lauryl sulfate, reinforced emulsion and fiber powder on the performance of the prepared porous filter material water purifier
[0044] Sodium carbonate, phosphogypsum and blast furnace slag are mixed in a mass ratio of 25:75:100, mixed and ground into powder to obtain carbon phosphorus ash slag mixed powder. The carbon phosphorus ash slag mixed powder is calcined to obtain a calcined mixed powder, wherein the calcination temperature is 1150°C and the calcination time is 4.5 hours. Silane coupling agent KH-590 and silicone acrylic emulsion are mixed in a mass ratio of 25:100, stirred evenly, and a reinforced emulsion is obtained. Polyester fiber powder and calcined mixed powder are mixed in a mass ratio of 2.5:100, stirred evenly, and fiber powder is obtained. According to the mass ratio of 0.75:15:100, 1:15:100, 1.25:15:100, 1.5:2.5:100, 1.5:3:100, 1.5:4:100, 1.5:5:100, 3.5:5:100, 5.5:5:100, 1.5:10:100, 3.5:10:100, 5.5:10:100, 1.5:15:100, 3.5:15:100, 5.5:15:100, 5.5:17.5:100, Sodium lauryl sulfate, reinforcing emulsion and fiber powder are mixed at a ratio of 5.5:20:100, 5.5:22.5:100, 6:15:100, 6.5:15:100 and 7:15:100, and then water is added to the mixture at a liquid-to-solid ratio of 0.45:1 mL / g, followed by high-speed stirring to obtain a foaming slurry, which is poured into a mold for molding and steam-cured to obtain a porous filter material, wherein the stirring rate is 1440 rpm, the stirring time is 12.5 minutes, the steam curing temperature is 360°C, and the curing time is 6 hours.
[0045] The landfill leachate purification test, COD concentration detection and COD adsorption capacity calculation, mercury ion concentration detection and adsorption capacity calculation are all the same as in Example 1. The COD and mercury ion adsorption capacity results are shown in Table 3.
[0046] Table 3 Effect of the mass ratio of sodium dodecyl sulfate, reinforced emulsion and fiber powder on the performance of the prepared porous filter media water purifier
[0047]
[0048] It can be seen from Table 3 that when the mass ratio of sodium dodecyl sulfate, reinforced emulsion and fiber powder is less than 1.5:5:100 (such as in Table 3, the mass ratio of sodium dodecyl sulfate, reinforced emulsion and fiber powder = 1.25:15:100, 1:15:100, 0.75:15:100, 1.5:4:100, 1.5:3:100, 1.5:2.5:100 and lower ratios not listed in Table 3), less sodium dodecyl sulfate and reinforced emulsion are added, and the reaction of sodium dodecyl sulfate, reinforced emulsion and fiber powder is not sufficient, resulting in the COD and mercury ion adsorption capacity of the prepared porous filter material being significantly reduced with the reduction of the mass ratio of sodium dodecyl sulfate, reinforced emulsion and fiber powder. When the mass ratio of sodium dodecyl sulfate, reinforcing emulsion and fiber powder is equal to 1.5~5.5:5~15:100 (as in Table 3, the mass ratio of sodium dodecyl sulfate, reinforcing emulsion and fiber powder is 1.5:5:100, 3.5:5:100, 5.5:5:100, 1.5:10:100, 3.5:10:100, 5.5:10:100, 1.5:15:100, 3.5:15:100, 5.5:15:100), sodium dodecyl sulfate, reinforcing emulsion and fiber powder are mixed, and water is added. Sodium dodecyl sulfate forms micelles in water and forms an adsorption film on the gas-liquid interface, thereby reducing the surface tension and quickly forming stable foam under high-speed stirring conditions, so that the slurry foams. The fiber powder undergoes a hydration reaction after contacting water to generate a silicate gel mixed with ettringite and calcium iron phosphate-based materials. The hydrophilic groups of sodium dodecyl sulfate react with the active mineral components in the fiber powder to digest and precipitate free calcium and magnesium oxides, which are then mixed into the silicate gel. The mercapto-loaded copolymers and acrylic monomers in the reinforced emulsion can react with iron, magnesium, and calcium cations to form an organosilicon complex mixture, which is then mixed into the silicate gel. During the steam curing process, the hydrophobic groups of sodium dodecyl sulfate can further react with acrylic monomers to induce the formation of copolymers, which encapsulate the hardened silicate hydration products. Ultimately, the COD adsorption capacity of the prepared porous filter materials is greater than 1587.36 mg / g, and the mercury ion adsorption capacity is greater than 95 mg / g. When the mass ratio of sodium dodecyl sulfate, reinforced emulsion and fiber powder is greater than 5.5:15:100 (as in Table 3, the mass ratio of sodium dodecyl sulfate, reinforced emulsion and fiber powder = 5.5:17.5:100, 5.5:20:100, 5.5:22.5:100, 6:15:100, 6.5:15:100, 7:15:100 and higher ratios not listed in Table 3), sodium dodecyl sulfate and reinforced emulsion are added excessively, and the material reaction is unbalanced, resulting in the COD and mercury ion adsorption capacity of the prepared porous filter material being significantly reduced with the further increase of the mass ratio of sodium dodecyl sulfate, reinforced emulsion and fiber powder.Therefore, in summary, considering the benefits and costs, when the mass ratio of sodium dodecyl sulfate, reinforcing emulsion and fiber powder is equal to 1.5~5.5:5~15:100, it is most conducive to improving the adsorption performance of the prepared porous filter material.
[0049] Comparative example of the effects of different processes on the performance of porous filter media water purifiers
[0050] The process of the present invention is as follows: sodium carbonate, phosphogypsum and blast furnace slag are mixed in a mass ratio of 25:75:100, mixed and ground into powder to obtain carbon phosphorus ash slag mixed powder. The carbon phosphorus ash slag mixed powder is calcined to obtain a calcined mixed powder, wherein the calcination temperature is 1150°C and the calcination time is 4.5 hours. Silane coupling agent KH-590 and silicone acrylic emulsion are mixed in a mass ratio of 25:100, stirred evenly, and a reinforced emulsion is obtained. Polyester fiber powder and calcined mixed powder are mixed in a mass ratio of 2.5:100, stirred evenly, and fiber powder is obtained. Sodium lauryl sulfate, reinforcing emulsion and fiber powder are mixed in a mass ratio of 5.5:15:100, and then water is added to the mixture in a liquid-to-solid ratio of 0.45:1 mL / g, followed by high-speed stirring to obtain a foaming slurry, which is poured into a mold for molding and steam-cured to obtain a porous filter material, wherein the stirring rate is 1440 rpm, the stirring time is 12.5 minutes, the steam curing temperature is 360°C, and the curing time is 6 hours.
[0051] Comparative process 1: Sodium carbonate, phosphogypsum, and blast furnace slag are mixed in a mass ratio of 25:75:100, mixed, and ground into powder to obtain a carbon phosphorus ash slag mixed powder. The carbon phosphorus ash slag mixed powder is calcined to obtain a calcined mixed powder, wherein the calcination temperature is 1150°C and the calcination time is 4.5 hours. Polyester fiber powder and calcined mixed powder are mixed in a mass ratio of 2.5:100, stirred evenly, and fiber mixed powder is obtained. Sodium dodecyl sulfate, silicone acrylic emulsion, and fiber mixed powder are mixed in a mass ratio of 5.5:15:100, and then water is added to the mixture at a liquid-solid ratio of 0.45:1mL / g, followed by high-speed stirring to obtain a foaming slurry poured into a mold for molding, steam curing, and a porous filter material is obtained, wherein the stirring rate is 1440rpm, the stirring time is 12.5 minutes, the steam curing temperature is 360°C, and the curing time is 6 hours.
[0052] Comparative process 2: Calcine the blast furnace slag to obtain calcined powder, wherein the calcination temperature is 1150°C and the calcination time is 4.5 hours. Mix silane coupling agent KH-590 and silicone-acrylic emulsion in a mass ratio of 25:100, stir evenly, and obtain a reinforced emulsion. Mix polyester fiber powder and calcined powder in a mass ratio of 2.5:100, stir evenly, and obtain fiber powder. Sodium lauryl sulfate, reinforced emulsion and fiber powder are mixed in a mass ratio of 5.5:15:100, and then water is added to the mixture in a liquid-solid ratio of 0.45:1mL / g, followed by high-speed stirring to obtain a foaming slurry poured into a mold for molding, steam curing, and a porous filter material is obtained, wherein the stirring rate is 1440rpm, the stirring time is 12.5 minutes, the steam curing temperature is 360°C, and the curing time is 6 hours.
[0053] The landfill leachate purification test, COD concentration detection and COD adsorption capacity calculation, mercury ion concentration detection and adsorption capacity calculation are all the same as in Example 1. The COD and mercury ion adsorption capacity results are shown in Table 4.
[0054] Table 4 Effects of different processes on the performance of the prepared porous filter media water purifier
[0055]
[0056] As shown in Table 4, the COD and mercury ion adsorption capacity of the porous filter material water purifier prepared by the process of the present invention are significantly higher than those of the comparative process 1 and the comparative process 2 and higher than the sum of the two.
Claims
1. A method for preparing a porous filter material using blast furnace slag, characterized in that: The following steps are involved: (1) mixing sodium carbonate, phosphogypsum and blast furnace slag, grinding them into powder, and obtaining a carbon-phosphorus ash-slag mixed powder; calcining the carbon-phosphorus ash-slag mixed powder to obtain a calcined mixed powder; The mass ratio of the sodium carbonate, phosphogypsum and blast furnace slag is 5-25:25-75:100; (2) Mixing the silane coupling agent and the silicone-acrylic emulsion, stirring evenly, and obtaining a reinforced emulsion; The mass ratio of the silane coupling agent to the silicone-acrylic emulsion is 5-25:100; (3) mixing the polyester fiber powder and the calcined mixed powder prepared in step (1), stirring evenly to obtain fiber-mixed powder; (4) mixing sodium lauryl sulfate, the strengthening emulsion prepared in step (2) and the fiber powder prepared in step (3), adding water to the mixture, and stirring at high speed to obtain a foaming slurry; The mass ratio of the sodium lauryl sulfate, the strengthening emulsion and the fiber powder is 1.5-5.5:5-15:100; (5) pouring the foaming slurry prepared in step (4) into a mold for molding, and steam curing to obtain a porous filter material.
2. The method for preparing porous filter material using blast furnace slag according to claim 1, characterized in that: The calcination temperature in step (1) is 850-1150° C., and the calcination time is 1.5-4.5 hours.
3. The method for preparing porous filter material using blast furnace slag according to claim 1, characterized in that: The silane coupling agent in step (2) is KH-590.
4. The method for preparing porous filter material using blast furnace slag according to claim 1, characterized in that: The mass ratio of the polyester fiber powder to the calcined mixed powder in step (3) is 0.5-2.5:
100.
5. The method for preparing porous filter material using blast furnace slag according to claim 1, characterized in that: In step (4), the liquid-to-solid ratio of water to the mixed material is 0.25-0.45:1 mL / g; the stirring rate is 360-1440 rpm, and the stirring time is 2.5-12.5 minutes.
6. The method for preparing porous filter material using blast furnace slag according to claim 1, characterized in that: The steam curing temperature in step (5) is 180-360° C., and the curing time is 2-6 hours.
7. The porous filter material prepared by the method according to any one of claims 1 to 6.
8. Use of the porous filter material according to claim 7 in purifying landfill leachate or sewage.
9. The use according to claim 8, characterized in that: The sewage contains mercury ions.
Citation Information
Patent Citations
Slag based mesoporous material and preparation method thereof
CN104163615A
Lithium slag unfired ceramsite filter material and preparation method thereof
CN117164319A