A type of concrete containing industrial solid waste steel slag and its preparation process

By adding zirconium oxide and molybdenum phosphide to concrete and combining it with polyurethane-modified acrylic emulsion coating granulation technology, the problems of flexural strength and abrasion resistance of concrete containing industrial solid waste have been solved, enabling the application of high-performance concrete.

CN118459176BActive Publication Date: 2026-11-17LANGFANG HENGDE NEW MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410803134.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-20
Publication Date
2026-11-17
Estimated Expiration
2044-06-20

AI Technical Summary

Technical Problem

Existing concrete containing industrial solid waste has low flexural strength and poor wear resistance, which limits its application in road and building engineering.

Method used

By adding zirconium oxide and molybdenum phosphide to concrete, and combining them with polyurethane-modified acrylic emulsion, adjusting their mass ratio, and then coating and granulating them, functional fillers are formed to improve the flexural strength and wear resistance of concrete.

Benefits of technology

It significantly improves the flexural strength and wear resistance of concrete containing industrial solid waste steel slag, meeting the needs of road and building engineering.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

This invention relates to the field of building materials technology, and proposes a concrete containing industrial solid waste steel slag and its preparation method. The concrete comprises the following components by weight: 85-95 parts cement, 25-35 parts industrial solid waste, 12-30 parts functional filler, 1-1.5 parts water-reducing agent, and 10-15 parts water; the functional filler includes zirconium oxide and molybdenum phosphide. This technical solution solves the problems of low flexural strength and poor wear resistance in existing concrete technologies.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of building materials technology, specifically to a type of concrete containing industrial solid waste steel slag and its preparation process. Background Technology

[0002] With the development of road and building construction, the market demand for cement concrete is also increasing. To adapt to the concept of green environmental protection, industrial solid waste can be utilized and transformed into valuable materials in concrete. However, current concrete containing industrial solid waste still suffers from low flexural strength and poor wear resistance. Therefore, developing concrete with high flexural strength and excellent wear resistance containing industrial solid waste will play a positive role in the resource utilization of industrial solid waste such as steel slag and fly ash, and in the application of concrete in road and building construction. Summary of the Invention

[0003] This invention proposes a concrete containing industrial solid waste steel slag and its preparation process, which solves the problems of low flexural strength and poor wear resistance of concrete in related technologies.

[0004] The technical solution of the present invention is as follows: This invention proposes a concrete containing industrial solid waste steel slag, comprising the following components by weight: 85-95 parts cement, 25-35 parts industrial solid waste, 12-30 parts functional filler, 1-1.5 parts water-reducing agent, and 10-15 parts water. The functional filler comprises zirconium oxide and molybdenum phosphide.

[0005] As a further technical solution, the mass ratio of zirconium oxide to molybdenum phosphide is 9:1~6.

[0006] In this invention, by adjusting the mass ratio of zirconium oxide and molybdenum phosphide to 9:1~6, the flexural strength and wear resistance of concrete containing industrial solid waste steel slag are further improved.

[0007] As a further technical solution, the components of the functional filler also include polyurethane-modified acrylic emulsion.

[0008] In this invention, in addition to adding zirconium oxide and molybdenum phosphide to the concrete, a polyurethane-modified acrylic emulsion is also introduced, which further improves the wear resistance and flexural strength of concrete containing industrial solid waste steel slag.

[0009] As a further technical solution, the combined mass of the zirconium oxide and molybdenum phosphide is 0.5 to 1 times the mass of the polyurethane-modified acrylic emulsion.

[0010] In this invention, the combined mass of zirconium oxide and molybdenum phosphide is limited to 0.5 to 1 times the mass of polyurethane-modified acrylic emulsion, which further improves the wear resistance and flexural strength of concrete containing industrial solid waste steel slag.

[0011] As a further technical solution, the preparation method of the functional filler includes the following steps: stirring and mixing zirconium oxide, molybdenum phosphide and polyurethane modified acrylic emulsion, granulating, and obtaining the functional filler.

[0012] In this invention, polyurethane-modified acrylic emulsion is used to coat and granulate zirconium oxide and molybdenum phosphide, which further improves the flexural strength and wear resistance of concrete containing industrial solid waste steel slag.

[0013] As a further technical solution, the industrial solid waste includes steel slag and fly ash; the mass ratio of the steel slag and fly ash is 4:1 to 3:2.

[0014] As a further technical solution, the particle size of the functional filler is 0.05~0.1mm.

[0015] As a further technical solution, the water-reducing agent is one or both of sulfonate-type water-reducing agents and fatty alcohol-type waterproofing agents.

[0016] As a further technical solution, the zirconium oxide has a particle size of 10~15μm.

[0017] This invention also proposes a process for preparing concrete containing industrial solid waste steel slag, comprising the following steps: The components in the specified weight proportions are mixed to obtain concrete containing industrial solid waste steel slag.

[0018] The working principle and beneficial effects of this invention are as follows: In this invention, zirconium oxide and molybdenum phosphide are added to concrete together, which has a synergistic strengthening effect. This not only significantly improves the flexural strength of concrete containing industrial solid waste steel slag, but also improves its wear resistance. Detailed Implementation

[0019] The technical solutions of the present invention will be clearly and completely described below with reference to the embodiments of the present invention. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those of ordinary skill in the art without creative effort are within the scope of protection of the present invention.

[0020] In the following examples and comparative examples, the cement was ordinary Portland cement PO 32.5; the molybdenum phosphide had a purity of 99.9% and was purchased from Shanghai Delta New Materials Co., Ltd.; the polyurethane modified acrylic emulsion was model PUA2922; the steel slag had an average particle size of 0.2 mm and was composed of the following components by mass percentage: CaO 47.5%, SiO2 18.3%, Al2O3 3.2%, MnO 3.2%, MgO 9.0%, TiO2 1.35%, Fe2O3 17.2%, Na2O 0.1%, with the balance being unavoidable impurities; and the fly ash was grade I fly ash.

[0021] Example 1 Concrete containing industrial solid waste steel slag comprises the following components in parts by weight: 85 parts cement, 20 parts steel slag, 5 parts fly ash, 11.4 parts zirconium oxide with a particle size of 10 μm, 0.6 parts molybdenum phosphide, 1 part sodium lignosulfonate, and 10 parts water. The preparation process of concrete containing industrial solid waste steel slag includes the following steps: The components of concrete containing industrial solid waste steel slag are mixed to obtain concrete containing industrial solid waste steel slag.

[0022] Example 2 Concrete containing industrial solid waste steel slag comprises the following components by weight: 90 parts cement, 21 parts steel slag, 14 parts fly ash, 17.1 parts zirconium oxide with a particle size of 10 μm, 0.9 parts molybdenum phosphide, 1.2 parts sodium lignosulfonate, and 12 parts water. The preparation process of concrete containing industrial solid waste steel slag includes the following steps: The components of concrete containing industrial solid waste steel slag are mixed to obtain concrete containing industrial solid waste steel slag.

[0023] Example 3 Concrete containing industrial solid waste steel slag comprises the following components in parts by weight: 95 parts cement, 20 parts steel slag, 5 parts fly ash, 28.4 parts zirconium oxide with a particle size of 15 μm, 1.6 parts molybdenum phosphide, 1.5 parts sodium lignosulfonate, and 15 parts water. The preparation process of concrete containing industrial solid waste steel slag includes the following steps: The components of concrete containing industrial solid waste steel slag are mixed to obtain concrete containing industrial solid waste steel slag.

[0024] Example 4 The difference between this embodiment and embodiment 3 is only that the concrete containing industrial solid waste steel slag includes the following components by weight: 95 parts cement, 20 parts steel slag, 5 parts fly ash, 16.9 parts zirconium oxide with a particle size of 15μm, 13.1 parts molybdenum phosphide, 1.5 parts sodium lignosulfonate, and 15 parts water.

[0025] Example 5 The only difference between this embodiment and Embodiment 3 is that the concrete containing industrial solid waste steel slag includes the following components by weight: 95 parts cement, 20 parts steel slag, 5 parts fly ash, 27 parts zirconium oxide with a particle size of 15 μm, 3 parts molybdenum phosphide, 1.5 parts sodium lignosulfonate, and 15 parts water.

[0026] Example 6 The difference between this embodiment and embodiment 3 is only that the concrete containing industrial solid waste steel slag includes the following components by weight: 95 parts cement, 20 parts steel slag, 5 parts fly ash, 18 parts zirconium oxide with a particle size of 15 μm, 12 parts molybdenum phosphide, 1.5 parts sodium lignosulfonate, and 15 parts water.

[0027] Example 7 The only difference between this embodiment and Embodiment 6 is that the concrete containing industrial solid waste steel slag includes the following components by weight: 95 parts cement, 20 parts steel slag, 5 parts fly ash, 10.8 parts zirconium oxide with a particle size of 15 μm, 7.2 parts molybdenum phosphide, 12 parts polyurethane modified acrylic emulsion, 1.5 parts sodium lignosulfonate, and 15 parts water.

[0028] Example 8 The only difference between this embodiment and embodiment 7 is that the concrete containing industrial solid waste steel slag includes the following components by weight: 95 parts cement, 20 parts steel slag, 5 parts fly ash, 10.8 parts zirconium oxide with a particle size of 15 μm, 7.2 parts molybdenum phosphide, 12 parts polyurethane modified acrylic emulsion, 1.5 parts sodium lignosulfonate, and 15 parts water. The preparation method of the functional filler includes the following steps: stirring and mixing zirconium oxide, molybdenum phosphide and polyurethane modified acrylic emulsion, granulating, to obtain a functional filler with a particle size of 0.05 mm; The preparation process of concrete containing industrial solid waste steel slag includes the following steps: The functional filler is mixed with the remaining components of concrete containing industrial solid waste steel slag to obtain concrete containing industrial solid waste steel slag.

[0029] Example 9 The only difference between this embodiment and Embodiment 8 is that the concrete containing industrial solid waste steel slag includes the following components by weight: 95 parts cement, 20 parts steel slag, 5 parts fly ash, 3 parts zirconium oxide with a particle size of 15 μm, 2 parts molybdenum phosphide, 25 parts polyurethane modified acrylic emulsion, 1.5 parts sodium lignosulfonate, and 15 parts water.

[0030] Example 10 The only difference between this embodiment and embodiment 8 is that the concrete containing industrial solid waste steel slag includes the following components by weight: 95 parts cement, 20 parts steel slag, 5 parts fly ash, 6 parts zirconium oxide with a particle size of 15 μm, 4 parts molybdenum phosphide, 20 parts polyurethane modified acrylic emulsion, 1.5 parts sodium lignosulfonate, and 15 parts water.

[0031] Example 11 The difference between this embodiment and embodiment 8 is only that the concrete containing industrial solid waste steel slag includes the following components by weight: 95 parts cement, 20 parts steel slag, 5 parts fly ash, 9 parts zirconium oxide with a particle size of 15 μm, 6 parts molybdenum phosphide, 15 parts polyurethane modified acrylic emulsion, 1.5 parts sodium lignosulfonate, and 15 parts water.

[0032] Example 12 The difference between this embodiment and Embodiment 11 is only that the preparation method of the functional filler includes the following steps: stirring and mixing zirconium oxide, molybdenum phosphide and polyurethane modified acrylic emulsion, granulating, to obtain a functional filler with a particle size of 0.1 mm.

[0033] Comparative Example 1 The only difference between this comparative example and Example 3 is that the concrete contains industrial solid waste steel slag, which includes the following components by weight: 95 parts cement, 20 parts steel slag, 5 parts fly ash, 1.5 parts sodium lignosulfonate, and 15 parts water.

[0034] Comparative Example 2 The only difference between this comparative example and Example 3 is that the concrete contains industrial solid waste steel slag, which includes the following components by weight: 95 parts cement, 20 parts steel slag, 5 parts fly ash, 25 parts zirconium oxide with a particle size of 15 μm, 1.5 parts sodium lignosulfonate, and 15 parts water.

[0035] Comparative Example 3 The only difference between this comparative example and Example 3 is that the concrete contains industrial solid waste steel slag, and includes the following components by weight: 95 parts cement, 20 parts steel slag, 5 parts fly ash, 25 parts molybdenum phosphide, 1.5 parts sodium lignosulfonate, and 15 parts water.

[0036] Comparative Example 4 The only difference between this comparative example and Example 3 is that the concrete contains industrial solid waste steel slag, which includes the following components by weight: 95 parts cement, 20 parts steel slag, 5 parts fly ash, 23.7 parts zirconium oxide with a particle size of 15 μm, 1.3 parts molybdenum oxide, 1.5 parts sodium lignosulfonate, and 15 parts water.

[0037] The concrete prepared in Examples 1-12 and Comparative Examples 1-4 were cured in a standard curing room for 28 days according to the method in GB / T 50081-2019 to obtain standard specimens of 150mm×150mm×600mm, and then the flexural strength was tested. The abrasion test was conducted on the concrete prepared in Examples 1-12 and Comparative Examples 1-4, respectively, according to the method in JTG 3420-2020 "Technical Guidelines for Construction of Cement Concrete Pavement of Highway". The test results are shown in Table 1 below.

[0038] Table 1. Test results of abrasion resistance and flexural strength

[0039] Compared with Comparative Examples 1-4, the concrete prepared in Examples 1-12 had lower abrasion and higher flexural strength, indicating that adding zirconium oxide and molybdenum phosphide to concrete can significantly improve the flexural strength and abrasion resistance of concrete.

[0040] Compared with Examples 3-4, the concrete prepared in Examples 5-6 has lower abrasion loss and higher flexural strength, indicating that by limiting the mass ratio of zirconium oxide and molybdenum phosphide to 9:1-6, the flexural strength and abrasion resistance of concrete can be further improved.

[0041] Compared with Example 6, the concrete prepared in Example 7 has lower abrasion and higher flexural strength, indicating that by adding polyurethane-modified acrylic emulsion to the concrete in addition to adding zirconium oxide and molybdenum phosphide, the abrasion resistance and flexural strength of the concrete can be further improved.

[0042] Compared with Example 7, the concrete prepared in Example 8 has lower abrasion loss and higher flexural strength, indicating that the polyurethane-modified acrylic emulsion can further improve the flexural strength and abrasion resistance of concrete by coating and granulating zirconium oxide and molybdenum phosphide.

[0043] Compared with Examples 8-9, the concrete prepared in Examples 10-12 has lower abrasion and higher flexural strength, indicating that limiting the mass of zirconium oxide and molybdenum phosphide to 0.5-1 times the mass of polyurethane-modified acrylic emulsion can further improve the abrasion resistance and flexural strength of concrete containing industrial solid waste steel slag.

[0044] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A concrete containing industrial solid waste steel slag, characterized by, The components include cement 85-95 parts, industrial solid waste 25-35 parts, functional filler 12-30 parts, water reducing agent 1-1.5 parts, and water 10-15 parts by weight; The components of the functional filler include zirconium oxide and molybdenum phosphide; the mass ratio of the zirconium oxide and the molybdenum phosphide is 9:1-6; the industrial solid waste includes steel slag and fly ash; the mass ratio of the steel slag and the fly ash is 4:1-3:

2.

2. The concrete containing industrial solid waste steel slag according to claim 1, characterized in that, The components of the functional filler further include polyurethane modified acrylic emulsion.

3. The concrete containing industrial solid waste steel slag according to claim 2, characterized by, The mass of the zirconium oxide and the molybdenum phosphide is 0.5-1 times the mass of the polyurethane modified acrylic emulsion.

4. The concrete containing industrial solid waste steel slag according to claim 3, characterized by, The preparation method of the functional filler includes the following steps: stirring and mixing zirconium oxide, molybdenum phosphide, and polyurethane modified acrylic emulsion, and granulating to obtain the functional filler.

5. The concrete containing industrial solid waste steel slag according to claim 4, characterized by, The particle size of the functional filler is 0.05-0.1 mm.

6. The concrete containing industrial solid waste steel slag according to claim 1, characterized by, The water reducing agent is a sulfonate type water reducing agent.

7. The concrete containing industrial solid waste steel slag according to claim 1, characterized in that, The particle size of the zirconium oxide is 10-15 μm.

8. The preparation process of concrete containing industrial solid waste steel slag according to any one of claims 1-7, characterized in that, The method includes the following steps: The components by weight are mixed to obtain concrete containing industrial solid waste steel slag. The method includes the following steps: The components by weight are mixed to obtain concrete containing industrial solid waste steel slag.

Citation Information

Patent Citations

  • Steel scoria concrete tile pipe and method for preparing same

    CN101289303A

  • Asphalt concrete filler and preparation process of asphalt concrete

    CN112358230A