A thermal insulation ceramic composite board and preparation method thereof

Through the ceramic bottom layer and surface layer of a specific composition, combined with ball milling and firing processes, the deformation, construction difficulty and cost problems of ceramic composite panels are solved, and a ceramic composite panel that is lightweight, thermal insulation, fireproof and mechanically strong is achieved, improving its Impact resistance and durability.

CN118459209BActive Publication Date: 2024-10-11FUJIAN JINJIANG SINONG CONSTR MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410936066.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-11
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

Ceramic composite panels face problems such as deformation and cracking, construction difficulty, high cost, durability and maintenance during production and application. In particular, UV resistance and freeze-thaw cycle resistance need to be considered when used outdoors.

Method used

The specific composition of the ceramic bottom layer and ceramic surface layer is used, including raw materials such as medical stone, perlite powder, diatomaceous earth, kaolin, bentonite and titanium dioxide, and the thermal insulation ceramic composite board is prepared through ball milling, spray drying and firing processes to optimize its Thermal conductivity, flexural strength and impact resistance.

Benefits of technology

The realization of lightweight, thermal insulation, fireproof and mechanically strong ceramic composite panels improves the overall performance of the material, enhances impact resistance and toughness, reduces internal defects, and improves the continuity and durability of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention provides a thermal insulation ceramic composite board and a preparation method thereof, belonging to the technical field of composite boards. The thermal insulation ceramic composite board comprises a ceramic bottom layer and a ceramic surface layer; the ceramic bottom layer comprises the following raw materials in mass fractions: 38-47 parts of medical stone, 12-35 parts of pearlite powder, 5-10 parts of alkali gangue, 12-22 parts of diatomite, 10-20 parts of kaolin, 5-15 parts of bentonite, 2-5 parts of sodium carbonate, 2-5 parts of fluorite, 5-8 parts of talc, 0.3-0.7 parts of potassium tripolyphosphate, 8-10 parts of aluminum hydroxide powder, 25-36 parts of ceramic particles, 5-10 parts of melamine, 1-2 parts of amyl acetate, and 1-3 parts of thioglycolic acid glyceride. The thermal insulation ceramic composite board has the advantages of light weight, good heat preservation, fire resistance and mechanical strength.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite boards, and in particular relates to a thermal insulation ceramic composite board and a preparation method thereof. Background Art

[0002] Ceramic composite board is a high-performance material that combines the high hardness, high temperature resistance, wear resistance, corrosion resistance and other characteristics of ceramic materials with the advantages of composite material technology. It is a composite material made by combining ceramic phase with another material (usually metal or polymer material) through certain process methods. The purpose of this material design is to improve the overall performance of the material, so that it has the excellent properties of ceramics and can overcome the shortcomings of traditional ceramics such as brittleness and difficulty in processing to a certain extent.

[0003] As a decorative material, ceramic composite panels have many advantages, such as excellent decorative effects, good physical properties, and environmental protection and non-radioactivity. However, they still face some technical challenges and problems in practical applications: (1) Deformation and cracking: Microcrystalline glass ceramic composite panels may deform or crack due to improper production process control, raw material quality differences, improper temperature and time control during heat treatment, etc. This requires manufacturers to strictly control the production process to ensure the uniformity and stability of the materials. (2) Construction difficulty: Although microcrystalline glass ceramic composite panels are easy to construct, they are heavier than traditional tiles, and have higher load-bearing requirements on walls or bases. They also require professional tools and skills for cutting and laying, which increases the construction difficulty and cost. (3) Cost issues: Compared with ordinary tiles, high-performance ceramic composite panels are usually more expensive due to their complex production process and high material costs, which may limit their application in some projects. (4) Durability and maintenance: Although ceramic composite panels are wear-resistant and scratch-resistant, during long-term use, especially for outdoor applications, their weather resistance properties such as UV resistance and freeze-thaw cycle resistance, as well as corresponding cleaning and maintenance measures, still need to be considered.

[0004] Therefore, there is an urgent need for a lightweight, heat-insulating, fire-resistant and mechanically strong thermal insulation ceramic composite board and a preparation method thereof, which has extremely high market value. Summary of the invention

[0005] The purpose of the present invention is to provide a thermal insulation ceramic composite board and a preparation method thereof.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] A thermal insulation ceramic composite board, comprising a ceramic bottom layer and a ceramic surface layer, wherein the thermal insulation ceramic composite board comprises a ceramic bottom layer and a ceramic surface layer; the ceramic bottom layer comprises the following raw materials in parts by weight: 38-47 parts of medical stone, 12-35 parts of perlite powder, 5-10 parts of alkali gangue, 12-22 parts of diatomaceous earth, 10-20 parts of kaolin, 5-15 parts of bentonite, 2-5 parts of sodium carbonate, 2-5 parts of fluorite, 5-8 parts of talc, 0.3-0.7 parts of potassium tripolyphosphate, 8-10 parts of aluminum hydroxide powder, 25-36 parts of ceramic particles, 5-10 parts of melamine, 1-2 parts of amyl acetate, and 1-3 parts of thioglycolic acid glyceride; the ceramic surface layer comprises the following raw materials in parts by mass: 80-90 parts of perlite powder, 1-10 parts of medical stone, 7-13 parts of diatomaceous earth, 20-35 parts of titanium dioxide, 1-2 parts of fluorite, 0.3-0.6 parts of potassium tripolyphosphate, and 1-3 parts of nano zirconium silicate.

[0008] Furthermore, the particle size of diatomaceous earth is 8-10 μm; the particle size of kaolin is 0.5-2 μm; and the particle size of bentonite is 4-6 μm.

[0009] Furthermore, the total weight fraction of the diatomaceous earth, kaolin and bentonite is ≥ 40 parts.

[0010] Furthermore, the mass ratio of diatomaceous earth, kaolin and bentonite is 18~22:10~15:12~15.

[0011] Furthermore, the titanium dioxide is a mixture of titanium dioxide A, titanium dioxide B and titanium dioxide C in a mass ratio of 1:1.2~1.5:0.4~0.7, the particle size of titanium dioxide A is 50~100nm; the particle size of titanium dioxide B is 150~200nm; and the particle size of titanium dioxide C is 200~300nm.

[0012] The present invention provides a method for preparing the thermal insulation ceramic composite board, comprising the following steps:

[0013] (1) The raw materials of the ceramic bottom layer and the raw materials of the ceramic surface layer are mixed with water, respectively, and subjected to ball milling, sieving, and aging treatment to obtain ceramic surface layer slurry and ceramic bottom layer slurry;

[0014] (2) spray drying and aging the ceramic surface layer slurry and the ceramic bottom layer slurry respectively to obtain a ceramic surface layer powder and a ceramic bottom layer powder;

[0015] (3) firstly coating the ceramic bottom layer powder, then backfilling the ceramic surface layer powder to obtain a preform, and then dry-pressing the preform to obtain a green body; drying, decorating and firing the green body to obtain a thermal insulation ceramic composite board.

[0016] Furthermore, the preform is pressed into a green body with a thickness of 20-40 mm.

[0017] Furthermore, the filling thickness of the ceramic bottom layer powder in the green body is 6-9 mm.

[0018] Furthermore, the water content of the ceramic surface layer powder and the ceramic bottom layer powder is 8.7-9.2 wt %.

[0019] Furthermore, the firing step includes: preheating and drying at 350-450°C for 10-15 min; continuing to bake and dry at 700-800°C for 25-30 min; continuing to heat at 1000-1020°C for 20-25 min; continuing to vitrify and melt at 1100-1130°C for 20-25 min; then expanding and foaming at 1140-1160°C for 25-30 min; keeping the foamed body at 600-900°C for 5-10 min; and finally keeping it at 100-200°C for 15-20 min.

[0020] It should be noted that the raw materials used in the present invention are all common raw materials for ceramic composite panels, and the raw materials are all commercially available, and there is no special restriction on the manufacturers.

[0021] Compared with the prior art, the advantages and beneficial effects of the present invention are as follows: the present invention provides a thermal insulation ceramic composite board and a preparation method thereof, wherein the thermal insulation ceramic composite board has the advantages of light weight, thermal insulation, fire resistance and good mechanical strength. The present invention uses a ceramic bottom layer and a ceramic surface layer composed of specific components to play a synergistic role with each other, thereby improving the thermal conductivity of the thermal insulation ceramic composite board. At the same time, the present invention uses diatomite, kaolin and bentonite of specific particle sizes, and the three synergistically improve the flexural strength of the thermal insulation ceramic composite board. The fine particles of diatomite, kaolin and bentonite can fill the pores of the ceramic matrix, reduce defects, and form finer and more uniform grains. At the same time, an appropriate amount of particles can also hinder crack propagation and play a toughening effect. Diatomite, kaolin and bentonite have good adhesion and bonding ability. When they are evenly distributed in the ceramic matrix, they can form a solid interface layer, which is tightly combined with the ceramic matrix through physical entanglement or chemical bonding, thereby improving the overall strength of the composite material. And when the total content is within a certain range, the porosity and density of the ceramic composite plate can be regulated, the microstructure can be optimized, and the mechanical properties of the material can be affected, including the improvement of flexural strength. Titanium dioxide particles of different particle sizes can fill the microscopic voids of the ceramic surface layer, optimize the microstructure, and form a tighter structural network. This optimization reduces internal defects and enhances the overall continuity of the material, thereby improving the ability of the surface layer to resist external impact. Titanium dioxide particles exist in the ceramic matrix as a heterogeneous phase and can form many tiny stress concentration points inside the material. When the material is impacted, these stress points can cause the impact energy to disperse instead of concentrating at a certain point, thereby reducing the formation and expansion of cracks and improving the impact resistance of the material. When titanium dioxide is sintered together with diatomaceous earth, kaolin, and bentonite, a more stable interface structure is formed at the grain boundary. These interfaces can act as a barrier to crack propagation, absorb and dissipate energy, and help improve the toughness and impact strength of the ceramic surface layer. DETAILED DESCRIPTION

[0022] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0023] Example 1

[0024] This embodiment provides a thermal insulation ceramic composite board, including a ceramic bottom layer and a ceramic surface layer.

[0025] The ceramic bottom layer comprises the following raw materials in parts by weight: 38 parts of medical stone, 12 parts of perlite powder, 5 parts of alkali gangue, 22 parts of diatomaceous earth, 10 parts of kaolin, 12 parts of bentonite, 2 parts of sodium carbonate, 2 parts of fluorite, 5 parts of talc, 0.3 parts of potassium tripolyphosphate, 8 parts of aluminum hydroxide powder, 25 parts of ceramic particles, 5 parts of melamine, 1 part of amyl acetate, and 1 part of thioglycolic acid glyceride;

[0026] The ceramic surface layer comprises the following raw materials in parts by mass: 80 parts of pearlite powder, 1 part of medical stone, 7 parts of diatomaceous earth, 20 parts of titanium dioxide, 1 part of fluorite, 0.3 parts of potassium tripolyphosphate, and 1 part of nano zirconium silicate.

[0027] The particle size of diatomaceous earth is 8~10μm; the particle size of kaolin is 0.5~2μm; the particle size of bentonite is 4~6μm.

[0028] The titanium dioxide is a mixture of titanium dioxide A, titanium dioxide B and titanium dioxide C in a mass ratio of 1:1.3:0.6, the particle size of titanium dioxide A is 50-100 nm; the particle size of titanium dioxide B is 150-200 nm; and the particle size of titanium dioxide C is 200-300 nm.

[0029] The method for preparing the thermal insulation ceramic composite plate comprises the following steps:

[0030] (1) The raw materials of the ceramic bottom layer and the raw materials of the ceramic surface layer are mixed with water, respectively, and subjected to ball milling, sieving, and aging treatment to obtain ceramic surface layer slurry and ceramic bottom layer slurry;

[0031] (2) spray drying and aging the ceramic surface layer slurry and the ceramic bottom layer slurry respectively to obtain a ceramic surface layer powder and a ceramic bottom layer powder;

[0032] (3) firstly coating the ceramic bottom layer powder, then backfilling the ceramic surface layer powder to obtain a preform, and then dry pressing the preform to obtain a green body; drying, decorating and firing the green body to obtain a thermal insulation ceramic composite board with a thickness of 41 mm.

[0033] The preform was pressed into a body having a thickness of 33 mm.

[0034] The filling thickness of the ceramic bottom layer powder in the green body is 10 mm.

[0035] The water content of the ceramic surface layer powder and the ceramic bottom layer powder is 9wt%.

[0036] The firing steps include: preheating and drying at 400°C for 15 minutes; continuing to bake and dry at 750°C for 30 minutes; continuing to heat at 1010°C for 20 minutes; continuing to vitrify and melt at 1120°C for 20 minutes; then expanding and foaming at 1150°C for 25 minutes; keeping the foamed body at 700°C for 10 minutes; and finally keeping it at 150°C for 20 minutes.

[0037] Example 2

[0038] This embodiment provides a thermal insulation ceramic composite board, including a ceramic bottom layer and a ceramic surface layer.

[0039] The ceramic bottom layer comprises the following raw materials in parts by mass: 47 parts of medical stone, 35 parts of pearlite powder, 10 parts of alkali gangue, 18 parts of diatomaceous earth, 10 parts of kaolin, 13 parts of bentonite, 5 parts of sodium carbonate, 5 parts of fluorite, 8 parts of talc, 0.7 parts of potassium tripolyphosphate, 10 parts of aluminum hydroxide powder, 36 parts of ceramic particles, 10 parts of melamine, 2 parts of amyl acetate, and 3 parts of thioglycolic acid glyceride; the ceramic surface layer comprises the following raw materials in parts by mass: 90 parts of pearlite powder, 10 parts of medical stone, 13 parts of diatomaceous earth, 35 parts of titanium dioxide, 2 parts of fluorite, 0.6 parts of potassium tripolyphosphate, and 3 parts of nano zirconium silicate.

[0040] The particle size of diatomaceous earth is 8~10μm; the particle size of kaolin is 0.5~2μm; the particle size of bentonite is 4~6μm.

[0041] The titanium dioxide is a mixture of titanium dioxide A, titanium dioxide B and titanium dioxide C in a mass ratio of 1:1.3:0.6, the particle size of titanium dioxide A is 50-100 nm; the particle size of titanium dioxide B is 150-200 nm; and the particle size of titanium dioxide C is 200-300 nm.

[0042] The method for preparing the thermal insulation ceramic composite plate comprises the following steps:

[0043] (1) The raw materials of the ceramic bottom layer and the raw materials of the ceramic surface layer are mixed with water, respectively, and subjected to ball milling, sieving, and aging treatment to obtain ceramic surface layer slurry and ceramic bottom layer slurry;

[0044] (2) spray drying and aging the ceramic surface layer slurry and the ceramic bottom layer slurry respectively to obtain a ceramic surface layer powder and a ceramic bottom layer powder;

[0045] (3) firstly coating the ceramic bottom layer powder, then backfilling the ceramic surface layer powder to obtain a preform, and then dry pressing the preform to obtain a green body; drying, decorating and firing the green body to obtain a thermal insulation ceramic composite board with a thickness of 41 mm.

[0046] The preform was pressed into a body having a thickness of 33 mm.

[0047] The filling thickness of the ceramic bottom layer powder in the green body is 10 mm.

[0048] The water content of the ceramic surface layer powder and the ceramic bottom layer powder is 9wt%.

[0049] The firing steps include: preheating and drying at 400°C for 15 minutes; continuing to bake and dry at 750°C for 30 minutes; continuing to heat at 1010°C for 20 minutes; continuing to vitrify and melt at 1120°C for 20 minutes; then expanding and foaming at 1150°C for 25 minutes; keeping the foamed body at 700°C for 10 minutes; and finally keeping it at 150°C for 20 minutes.

[0050] Comparative Example 1

[0051] The difference between this comparative example and Example 1 is that the proportions of diatomaceous earth, kaolin and bentonite are different.

[0052] A thermal insulation ceramic composite board comprises a ceramic bottom layer and a ceramic surface layer.

[0053] The ceramic bottom layer comprises the following raw materials in parts by weight: 38 parts of medical stone, 12 parts of perlite powder, 5 parts of alkali gangue, 5 parts of diatomaceous earth, 22 parts of kaolin, 17 parts of bentonite, 2 parts of sodium carbonate, 2 parts of fluorite, 5 parts of talc, 0.3 parts of potassium tripolyphosphate, 8 parts of aluminum hydroxide powder, 25 parts of ceramic particles, 5 parts of melamine, 1 part of amyl acetate, and 1 part of thioglycolic acid glyceride;

[0054] The ceramic surface layer comprises the following raw materials in parts by mass: 80 parts of pearlite powder, 1 part of medical stone, 7 parts of diatomaceous earth, 20 parts of titanium dioxide, 1 part of fluorite, 0.3 parts of potassium tripolyphosphate, and 1 part of nano zirconium silicate.

[0055] The particle size of diatomaceous earth is 8~10μm; the particle size of kaolin is 0.5~2μm; the particle size of bentonite is 4~6μm.

[0056] The titanium dioxide is a mixture of titanium dioxide A, titanium dioxide B and titanium dioxide C in a mass ratio of 1:1.3:0.6, the particle size of titanium dioxide A is 50-100 nm; the particle size of titanium dioxide B is 150-200 nm; and the particle size of titanium dioxide C is 200-300 nm.

[0057] The method for preparing the thermal insulation ceramic composite plate comprises the following steps:

[0058] (1) The raw materials of the ceramic bottom layer and the raw materials of the ceramic surface layer are mixed with water, respectively, and subjected to ball milling, sieving, and aging treatment to obtain ceramic surface layer slurry and ceramic bottom layer slurry;

[0059] (2) spray drying and aging the ceramic surface layer slurry and the ceramic bottom layer slurry respectively to obtain a ceramic surface layer powder and a ceramic bottom layer powder;

[0060] (3) firstly coating the ceramic bottom layer powder, then backfilling the ceramic surface layer powder to obtain a preform, and then dry pressing the preform to obtain a green body; drying, decorating and firing the green body to obtain a thermal insulation ceramic composite board with a thickness of 41 mm.

[0061] The preform was pressed into a body having a thickness of 33 mm.

[0062] The filling thickness of the ceramic bottom layer powder in the green body is 10 mm.

[0063] The water content of the ceramic surface layer powder and the ceramic bottom layer powder is 9wt%.

[0064] The firing steps include: preheating and drying at 400°C for 15 minutes; continuing to bake and dry at 750°C for 30 minutes; continuing to heat at 1010°C for 20 minutes; continuing to vitrify and melt at 1120°C for 20 minutes; then expanding and foaming at 1150°C for 25 minutes; keeping the foamed body at 700°C for 10 minutes; and finally keeping it at 150°C for 20 minutes.

[0065] Comparative Example 2

[0066] The difference between this comparative example and Example 1 is that the particle sizes of diatomaceous earth, kaolin and bentonite are different.

[0067] A thermal insulation ceramic composite board comprises a ceramic bottom layer and a ceramic surface layer.

[0068] The ceramic bottom layer comprises the following raw materials in parts by weight: 38 parts of medical stone, 12 parts of perlite powder, 5 parts of alkali gangue, 22 parts of diatomaceous earth, 10 parts of kaolin, 12 parts of bentonite, 2 parts of sodium carbonate, 2 parts of fluorite, 5 parts of talc, 0.3 parts of potassium tripolyphosphate, 8 parts of aluminum hydroxide powder, 25 parts of ceramic particles, 5 parts of melamine, 1 part of amyl acetate, and 1 part of thioglycolic acid glyceride;

[0069] The ceramic surface layer comprises the following raw materials in parts by mass: 80 parts of pearlite powder, 1 part of medical stone, 7 parts of diatomaceous earth, 20 parts of titanium dioxide, 1 part of fluorite, 0.3 parts of potassium tripolyphosphate, and 1 part of nano zirconium silicate.

[0070] The particle size of diatomaceous earth is 6~8μm; the particle size of kaolin is 3~5μm; the particle size of bentonite is 7~9μm.

[0071] The titanium dioxide is a mixture of titanium dioxide A, titanium dioxide B and titanium dioxide C in a mass ratio of 1:1.3:0.6, the particle size of titanium dioxide A is 50-100 nm; the particle size of titanium dioxide B is 150-200 nm; and the particle size of titanium dioxide C is 200-300 nm.

[0072] The method for preparing the thermal insulation ceramic composite plate comprises the following steps:

[0073] (1) The raw materials of the ceramic bottom layer and the raw materials of the ceramic surface layer are mixed with water, respectively, and subjected to ball milling, sieving, and aging treatment to obtain ceramic surface layer slurry and ceramic bottom layer slurry;

[0074] (2) spray drying and aging the ceramic surface layer slurry and the ceramic bottom layer slurry respectively to obtain a ceramic surface layer powder and a ceramic bottom layer powder;

[0075] (3) firstly coating the ceramic bottom layer powder, then backfilling the ceramic surface layer powder to obtain a preform, and then dry pressing the preform to obtain a green body; drying, decorating and firing the green body to obtain a thermal insulation ceramic composite board with a thickness of 41 mm.

[0076] The preform was pressed into a body having a thickness of 33 mm.

[0077] The filling thickness of the ceramic bottom layer powder in the green body is 10 mm.

[0078] The water content of the ceramic surface layer powder and the ceramic bottom layer powder is 9wt%.

[0079] The firing steps include: preheating and drying at 400°C for 15 minutes; continuing to bake and dry at 750°C for 30 minutes; continuing to heat at 1010°C for 20 minutes; continuing to vitrify and melt at 1120°C for 20 minutes; then expanding and foaming at 1150°C for 25 minutes; keeping the foamed body at 700°C for 10 minutes; and finally keeping it at 150°C for 20 minutes.

[0080] Comparative Example 3

[0081] The difference between this comparative example and Example 1 is that the titanium dioxide composition is different.

[0082] A thermal insulation ceramic composite board comprises a ceramic bottom layer and a ceramic surface layer.

[0083] The ceramic bottom layer comprises the following raw materials in parts by weight: 38 parts of medical stone, 12 parts of perlite powder, 5 parts of alkali gangue, 22 parts of diatomaceous earth, 10 parts of kaolin, 12 parts of bentonite, 2 parts of sodium carbonate, 2 parts of fluorite, 5 parts of talc, 0.3 parts of potassium tripolyphosphate, 8 parts of aluminum hydroxide powder, 25 parts of ceramic particles, 5 parts of melamine, 1 part of amyl acetate, and 1 part of thioglycolic acid glyceride;

[0084] The ceramic surface layer comprises the following raw materials in parts by mass: 80 parts of pearlite powder, 1 part of medical stone, 7 parts of diatomaceous earth, 20 parts of titanium dioxide, 1 part of fluorite, 0.3 parts of potassium tripolyphosphate, and 1 part of nano zirconium silicate.

[0085] The particle size of diatomaceous earth is 8~10μm; the particle size of kaolin is 0.5~2μm; the particle size of bentonite is 4~6μm.

[0086] The titanium dioxide is a mixture of titanium dioxide A, titanium dioxide B and titanium dioxide C in a mass ratio of 1:1:1, the particle size of titanium dioxide A is 200-300 nm; the particle size of titanium dioxide B is 10-50 nm; and the particle size of titanium dioxide C is 300-400 nm.

[0087] The method for preparing the thermal insulation ceramic composite plate comprises the following steps:

[0088] (1) The raw materials of the ceramic bottom layer and the raw materials of the ceramic surface layer are mixed with water, respectively, and subjected to ball milling, sieving, and aging treatment to obtain ceramic surface layer slurry and ceramic bottom layer slurry;

[0089] (2) spray drying and aging the ceramic surface layer slurry and the ceramic bottom layer slurry respectively to obtain a ceramic surface layer powder and a ceramic bottom layer powder;

[0090] (3) firstly coating the ceramic bottom layer powder, then backfilling the ceramic surface layer powder to obtain a preform, and then dry pressing the preform to obtain a green body; drying, decorating and firing the green body to obtain a thermal insulation ceramic composite board with a thickness of 41 mm.

[0091] The preform was pressed into a body having a thickness of 33 mm.

[0092] The filling thickness of the ceramic bottom layer powder in the green body is 10 mm.

[0093] The water content of the ceramic surface layer powder and the ceramic bottom layer powder is 9wt%.

[0094] The firing steps include: preheating and drying at 400°C for 15 minutes; continuing to bake and dry at 750°C for 30 minutes; continuing to heat at 1010°C for 20 minutes; continuing to vitrify and melt at 1120°C for 20 minutes; then expanding and foaming at 1150°C for 25 minutes; keeping the foamed body at 700°C for 10 minutes; and finally keeping it at 150°C for 20 minutes.

[0095] Comparative Example 4

[0096] The difference between this comparative example and Example 1 is that the proportions of diatomaceous earth, kaolin and bentonite are different.

[0097] A thermal insulation ceramic composite board comprises a ceramic bottom layer and a ceramic surface layer.

[0098] The ceramic bottom layer comprises the following raw materials in parts by weight: 38 parts of medical stone, 12 parts of perlite powder, 5 parts of alkali gangue, 12 parts of diatomaceous earth, 20 parts of kaolin, 12 parts of bentonite, 2 parts of sodium carbonate, 2 parts of fluorite, 5 parts of talc, 0.3 parts of potassium tripolyphosphate, 8 parts of aluminum hydroxide powder, 25 parts of ceramic particles, 5 parts of melamine, 1 part of amyl acetate, and 1 part of thioglycolic acid glyceride;

[0099] The ceramic surface layer comprises the following raw materials in parts by mass: 80 parts of pearlite powder, 1 part of medical stone, 7 parts of diatomaceous earth, 20 parts of titanium dioxide, 1 part of fluorite, 0.3 parts of potassium tripolyphosphate, and 1 part of nano zirconium silicate.

[0100] The particle size of diatomaceous earth is 8~10μm; the particle size of kaolin is 0.5~2μm; the particle size of bentonite is 4~6μm.

[0101] The titanium dioxide is a mixture of titanium dioxide A, titanium dioxide B and titanium dioxide C in a mass ratio of 1:1.3:0.6, the particle size of titanium dioxide A is 50-100 nm; the particle size of titanium dioxide B is 150-200 nm; and the particle size of titanium dioxide C is 200-300 nm.

[0102] The method for preparing the thermal insulation ceramic composite plate comprises the following steps:

[0103] (1) The raw materials of the ceramic bottom layer and the raw materials of the ceramic surface layer are mixed with water, respectively, and subjected to ball milling, sieving, and aging treatment to obtain ceramic surface layer slurry and ceramic bottom layer slurry;

[0104] (2) spray drying and aging the ceramic surface layer slurry and the ceramic bottom layer slurry respectively to obtain a ceramic surface layer powder and a ceramic bottom layer powder;

[0105] (3) firstly coating the ceramic bottom layer powder, then backfilling the ceramic surface layer powder to obtain a preform, and then dry pressing the preform to obtain a green body; drying, decorating and firing the green body to obtain a thermal insulation ceramic composite board with a thickness of 41 mm.

[0106] The preform was pressed into a body having a thickness of 33 mm.

[0107] The filling thickness of the ceramic bottom layer powder in the green body is 10 mm.

[0108] The water content of the ceramic surface layer powder and the ceramic bottom layer powder is 9wt%.

[0109] The firing steps include: preheating and drying at 400°C for 15 minutes; continuing to bake and dry at 750°C for 30 minutes; continuing to heat at 1010°C for 20 minutes; continuing to vitrify and melt at 1120°C for 20 minutes; then expanding and foaming at 1150°C for 25 minutes; keeping the foamed body at 700°C for 10 minutes; and finally keeping it at 150°C for 20 minutes.

[0110] Performance Testing

[0111] The performance tests were conducted on the composite boards of Examples 1-2 and Comparative Examples 1-4. The results are shown in Table 1.

[0112]

[0113] It can be seen from the above performance test results that the comprehensive performance of the ceramic composite board of Examples 1-2 is outstanding, which is mainly due to the synergistic effect of multiple components to improve the performance. However, the comparative example is significantly worse than the embodiment in the corresponding performance test because it does not adopt the necessary technical solution. The above experimental results further prove the importance of the technical solution defined in the present invention for its technical effect.

[0114] The above is a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A thermal insulation ceramic composite panel, characterized in that: The thermal insulation ceramic composite board includes a ceramic bottom layer and a ceramic surface layer; the ceramic bottom layer includes the following raw materials in parts by weight: 38 parts of medical stone, 12 parts of perlite powder, 5 parts of alkali gangue, 22 parts of diatomaceous earth, 10 parts of kaolin, 12 parts of bentonite, 2 parts of sodium carbonate, 2 parts of fluorite, 5 parts of talc, 0.3 parts of potassium tripolyphosphate, 8 parts of aluminum hydroxide powder, 25 parts of ceramic particles, 5 parts of melamine, 1 part of amyl acetate, and 1 part of thioglycolic acid glyceride; The ceramic surface layer comprises the following raw materials in parts by weight: 80 parts of perlite powder, 1 part of medical stone, 7 parts of diatomaceous earth, 20 parts of titanium dioxide, 1 part of fluorite, 0.3 parts of potassium tripolyphosphate, and 1 part of nano zirconium silicate; The particle size of diatomaceous earth is 8~10μm; the particle size of kaolin is 0.5~2μm; the particle size of bentonite is 4~6μm; The titanium dioxide is a mixture of titanium dioxide A, titanium dioxide B and titanium dioxide C in a mass ratio of 1:1.3:0.6, wherein the particle size of titanium dioxide A is 50-100 nm; the particle size of titanium dioxide B is 150-200 nm; and the particle size of titanium dioxide C is 200-300 nm; The method for preparing the thermal insulation ceramic composite plate comprises the following steps: (1) The raw materials of the ceramic bottom layer and the raw materials of the ceramic surface layer are mixed with water, respectively, and subjected to ball milling, sieving, and aging treatment to obtain ceramic surface layer slurry and ceramic bottom layer slurry; (2) spray drying and aging the ceramic surface layer slurry and the ceramic bottom layer slurry respectively to obtain a ceramic surface layer powder and a ceramic bottom layer powder; (3) first coating the ceramic bottom layer powder, then backfilling the ceramic surface layer powder to obtain a preform, and then dry pressing the preform to obtain a green body; drying, decorating, and firing the green body to obtain a thermal insulation ceramic composite board with a thickness of 41 mm; Pressing the preform into a body having a thickness of 33 mm; The filling thickness of the ceramic bottom layer powder in the green body is 10 mm; The moisture content of the ceramic surface layer powder and the ceramic bottom layer powder is 9wt%; The firing steps include: preheating and drying at 400°C for 15 minutes; continuing to bake and dry at 750°C for 30 minutes; continuing to heat at 1010°C for 20 minutes; continuing to vitrify and melt at 1120°C for 20 minutes; then expanding and foaming at 1150°C for 25 minutes; keeping the foamed body at 700°C for 10 minutes; and finally keeping it at 150°C for 20 minutes.