A method for preparing a magnetic core

By doping ferrocene-based polymer magnets with manganese-zinc ferrite and adding rare earth lanthanum and grain boundary strengtheners, the problems of insufficient magnetization strength and high magnetic loss of manganese-zinc ferrite cores in high-frequency and microwave frequency bands are solved. problem, achieving magnetic core materials with high saturation magnetization and low magnetic loss, which are suitable for high-frequency electronic equipment.

CN118459216BActive Publication Date: 2024-10-18NANTONG GUANYOUDA MAGNET
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410537453.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-12
Publication Date
2024-10-18
Estimated Expiration
2043-12-12

AI Technical Summary

Technical Problem

Existing manganese-zinc ferrite cores have insufficient magnetization strength and high magnetic loss in high-frequency and microwave frequency band applications, which cannot meet the needs of high-frequency electronic equipment and have electromagnetic wave interference problems.

Method used

Ferrocene-based polymer magnets are doped with manganese-zinc ferrite, and the nitrogen atoms in the bipyridine structure are coordinated with metal ions to form a tight bond. Rare earth lanthanum and grain boundary strengtheners are added during the preparation process to form a high-performance magnet. The resistivity of the grain boundary structure improves the magnetic properties.

Benefits of technology

It significantly improves the saturation magnetization and low magnetic loss of the magnetic core, enhances the electromagnetic performance in high-frequency and microwave frequency bands, reduces power loss, and broadens the scope of applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The invention relates to the technical field of manganese-zinc ferrite magnetic cores, and discloses a method for preparing the magnetic cores. A ferrocene-based polymer magnet containing a bipyridine structure has a coordination effect with metal ions in manganese-zinc ferrite, so that La 3+ Metal ions are doped into the molecular chain of the polymer magnet, which promotes a close combination of the two, thereby greatly improving the magnetic properties of the composite magnetic core; the grain boundary strengtheners CaCO3 and SiO2 will generate high-resistivity CaSiO3, which accumulates at high concentrations at the grain boundaries, increasing the grain boundary resistivity; Al2O3 generates a low-conductivity protective film under the action of high-temperature sintering, forming a shell-core structure, which increases the resistivity inside the grains. The increase in the resistivity of grain boundaries and grains effectively reduces the power loss of the material; the electromagnetic properties of ferrocene-based polymer magnets are very stable, and are suitable for the manufacture of many high-frequency and microwave electronic devices.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application with application number 2023116968806, application date December 12, 2023, and invention name “Preparation and Application of a Doped Manganese-Zinc Ferrite Core”. Technical Field

[0002] The invention relates to the technical field of manganese-zinc ferrite cores, in particular to a method for preparing a core. Background Art

[0003] In recent years, various electronic devices have been continuously developing in the direction of high frequency, integration, functionality and digitization. Electronic and electrical equipment have gradually been widely used in various fields of people's production and daily life. Manganese-zinc ferrite is a material with wide applications, large usage and low price. It has been widely used in a series of electronic devices such as switching power supply transformer cores, line output transformer cores in TV receivers and tape recorder heads. However, the magnetic permeability of a single ferrite material will decrease sharply with the increase of application frequency, and the magnetic loss will increase significantly. It is becoming increasingly difficult to develop electronic components in the direction of lightweight, miniaturization, miniaturization and multifunctionality. Therefore, seeking a new generation of lightweight, high permeability and low-loss magnetic materials has become a hot topic in current research and development.

[0004] The magnetic core is a magnetic material used in electronic devices such as power transformers, color TV transformers and switching power supplies. The magnetic core needs to transfer power by magnetization under high current or high current with DC bias field. Therefore, the higher the saturation flux density of the manganese-zinc ferrite core, the greater the transfer effect. However, the existing manganese-zinc ferrite core is generally prepared by the traditional oxide method, but the content of impurities such as aluminum oxide, sodium oxide and phosphorus pentoxide in oxides such as ferric oxide and manganese oxide on the market is relatively high, which easily leads to a decrease in the saturation flux density of the manganese-zinc ferrite core finally obtained, making the magnetic core product unable to meet the application requirements of high-power devices; at the same time, the widespread popularization of electronic equipment has brought great convenience to people's lives, but electromagnetic wave interference has also increased, especially high-frequency interference has become more and more serious, but the existing manganese-zinc-iron ferrite materials have narrow suppression bands and poor high-frequency filtering effects. Weaknesses are gradually exposed. In the field of filter applications, there are still many shortcomings, such as poor permeability characteristics and temperature characteristics under normal temperature conditions, low saturation flux density, and the core Curie temperature does not meet the requirements.

[0005] Compared with traditional manganese zinc ferrite, organic ferrocene-based polymer magnets have very stable electromagnetic properties in a wide temperature range and low magnetic loss under high-frequency microwaves, and are suitable for making many high-frequency and microwave electronic devices. The present invention synthesizes ferrocene-based polymer magnets, and the nitrogen atoms in the bipyridine structure can coordinate with the metal ions in the manganese zinc ferrite, so that La 3+Metal ions are doped into the molecular chains of polymer magnets, making the two tightly combined, which makes up for certain limitations of conventional ferrite cores in certain high-frequency and microwave frequency band applications, with high magnetization intensity and low power loss. Summary of the invention

[0006] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a method for preparing a magnetic core, which has the characteristics of high magnetization intensity and low loss.

[0007] The technical solution adopted by the present invention is:

[0008] A method for preparing a magnetic core, the magnetic core comprising the following components in parts by weight: 5-25 parts of ferrocene-based polymer magnet, 100 parts of manganese-zinc ferrite and 0.5-3 parts of polyethylene wax.

[0009] The preparation method is as follows: adding the above proportion of ferrocene-based polymer magnet, manganese zinc ferrite and polyethylene wax into a high-speed mixer, mixing them evenly at a rotation speed of 5000-8000 r / min, and then pressing and molding at 200-300 MPa to obtain a doped manganese zinc ferrite core.

[0010] Furthermore, the preparation method of the manganese-zinc ferrite is: adding 55-65 parts of iron oxide, 20-35 parts of manganese oxide, 5-15 parts of zinc oxide, 0.01-0.1 parts of lanthanum oxide and 0.1-0.5 parts of grain boundary strengthener by weight into a ball mill, performing a ball milling at a rotation speed of 200-300r / min for 8-16h, then adding it to a muffle furnace, pre-burning it at a temperature of 800-1000°C for 2-4h, cooling it to room temperature with the furnace, and then performing a secondary ball milling until the powder particle size is 5-10μm, and then pressing the mixed powder into a shape, and finally sintering it at 1300-1450°C for 3-5h, cooling it naturally, and obtaining manganese-zinc ferrite.

[0011] Furthermore, the grain boundary strengthener is any one of CaCO3, SiO2, and Al2O3.

[0012] Furthermore, the compression molding pressure is 15-20 MPa.

[0013] Furthermore, the preparation method of the ferrocene-based polymer magnet is:

[0014] (1) Add 100 parts by weight of 1,1′-ferrocenedicarboxylic acid, 85-110 parts by weight of thionyl chloride and 2-5 parts by weight of N,N-dimethylformamide to a reaction flask, stir to react, and after the reaction is completed, perform vacuum distillation to obtain 1,1′-ferrocenedicarboxylic acid chloride. The preparation process is as follows:

[0015]

[0016] (2) Add 1,1′-ferrocene dicarbonyl chloride and N,N-dimethylacetamide solvent to the reaction flask, stir evenly, then add [2,2'-bipyridine]-5,5'-diamine and triethylamine, stir and react. After the reaction is completed, add methanol, precipitate, filter, wash with deionized water until neutral, and dry to obtain ferrocene-based polymer magnet. The preparation process mechanism is as follows:

[0017]

[0018] Furthermore, in step (1), the reaction temperature is 80-100° C. and the reaction time is 3-8 h.

[0019] Furthermore, in the step (2), by weight, 1,1′-ferrocenyl dicarbonyl chloride is 100 parts, [2,2′-bipyridine]-5,5′-diamine is 50-70 parts, and triethylamine is 75-90 parts.

[0020] Furthermore, in step (2), the reaction is first carried out at 0-10°C for 1-4 hours, and then at 20-35°C for 4-8 hours.

[0021] By adopting the above technical solution, the beneficial effects of the present invention are:

[0022] According to the invention, 1,1′-ferrocene dicarboxylic acid is subjected to the action of thionyl chloride to obtain 1,1′-ferrocene dicarbonyl chloride, which is then polymerized with [2,2′-bipyridine]-5,5′-diamine to obtain a ferrocene-based polymer magnet; then, the raw materials of ferrite, such as iron oxide, manganese oxide and zinc oxide, are proportion-controlled, and rare earth lanthanum and a grain boundary strengthener are added to prepare manganese-zinc ferrite through processes such as ball milling, sintering and pressing molding; finally, the ferrocene-based polymer magnet, the manganese-zinc ferrite and lubricant polyethylene wax are mixed at high speed and pressed to obtain a doped manganese-zinc ferrite magnetic core.

[0023] Ferrocene-based polymer magnets containing bipyridine structures were synthesized using ferrocene dicarboxylic acid as raw material. The magnetic contribution mainly comes from the charge transfer of iron ions in ferrocene, and the mixed valence of divalent iron and trivalent iron is generated. The bipyridine nitrogen atom and conjugated benzene ring in the polymer magnet have coordination effects, making La 3+ The metal ions are doped into the molecular chain of the polymer magnet to promote the close combination of the two. After coordination, a lamellar structure is formed. A large range of conjugated system free electron self-selection coupling occurs between the layers. The appropriate amount of La 3+ Enter the octahedral structure of MnZn ferrite to replace Fe 3+ The excess rare earth La is adsorbed around the ferrite grain boundaries, exerting a certain pressure on the grain boundaries, thereby greatly improving the magnetic properties of the composite core.

[0024] The addition of grain boundary strengthener can reduce the power loss of the sample. During the sintering process of manganese-zinc ferrite, CaCO3 and SiO2 will generate high-resistivity CaSiO3, which accumulates at high concentrations at the grain boundaries, thereby increasing the grain boundary resistivity. Under the action of high-temperature sintering, Al2O3 can generate a low-conductivity protective film on the surface of the ferrite to form a shell-core structure, thereby increasing the resistivity inside the ferrite grains. The increase in the resistivity of grain boundaries and grains effectively reduces the power loss of the material.

[0025] Compared with manganese zinc ferrite, the magnetic properties of ferrocene-based polymer magnets are intrinsic. The ferrocene group in the magnet has very stable electromagnetic properties over a wide temperature range, and has low specific gravity and is easy to hot-press into shape. The high-frequency and microwave bands basically do not affect the structure of the ferrocene magnet, making it suitable for the manufacture of many high-frequency and microwave electronic devices, further broadening the application range of manganese zinc ferrite. DETAILED DESCRIPTION

[0026] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0027] Example 1

[0028] (1) Add 10 parts by weight of 1,1′-ferrocenedicarboxylic acid, 90 parts by weight of thionyl chloride and 0.3 parts by weight of N,N-dimethylformamide into a reaction flask, react at 90°C for 6 hours, and distill under reduced pressure to obtain 1,1′-ferrocenedicarboxylic acid chloride.

[0029] (2) Add 50 parts by weight of 1,1′-ferrocene dicarbonyl chloride and N,N-dimethylacetamide solvent to a reaction flask, stir evenly, then add 30 parts of [2,2′-bipyridine]-5,5′-diamine and 40 parts of triethylamine, stir and react, first at 5°C for 3 h and then at 25°C for 6 h, then add methanol to precipitate, filter, wash with deionized water until neutral, and dry to obtain a ferrocene-based polymer magnet.

[0030] (3) Add 60 parts by weight of iron oxide, 30 parts by weight of manganese oxide, 10 parts by weight of zinc oxide, 0.01 parts by weight of lanthanum oxide and 0.1 parts by weight of grain boundary strengthener CaCO3 into a ball mill, and perform a first ball milling at a rotation speed of 250 r / min for 12 h. Then, add the mixture into a muffle furnace, pre-sinter at 900°C for 3 h, cool to room temperature with the furnace, and then perform a second ball milling until the powder particle size is 8 μm. Then, press the mixed powder into a mold at a pressure of 18 MPa, and finally sinter at 1400°C for 4 h. Then, cool naturally to obtain manganese-zinc ferrite.

[0031] (4) Add 5 parts by weight of ferrocene-based polymer magnet, 100 parts by weight of manganese-zinc ferrite and 2 parts by weight of polyethylene wax into a high-speed mixer, mix them evenly at a speed of 7500 r / min, and then press them at 260 MPa to obtain a doped manganese-zinc ferrite core.

[0032] Example 2

[0033] (1) Add 100 parts by weight of 1,1′-ferrocenedicarboxylic acid, 110 parts by weight of thionyl chloride and 5 parts by weight of N,N-dimethylformamide into a reaction flask, react at 80°C for 8 hours, and distill under reduced pressure to obtain 1,1′-ferrocenedicarboxylic acid chloride.

[0034] (2) Add 100 parts by weight of 1,1′-ferrocene dicarbonyl chloride and N,N-dimethylacetamide solvent to a reaction flask, stir evenly, then add 70 parts of [2,2′-bipyridine]-5,5′-diamine and 90 parts of triethylamine, stir and react, first at 0°C for 4 h and then at 20°C for 8 h, then add methanol to precipitate, filter, wash with deionized water until neutral, and dry to obtain a ferrocene-based polymer magnet.

[0035] (3) Add 55 parts of iron oxide, 30 parts of manganese oxide, 15 parts of zinc oxide, 0.03 parts of lanthanum oxide and 0.1 parts of grain boundary strengthener SiO2 by weight into a ball mill, and perform a ball milling at a rotation speed of 300 r / min for 16 h. Then add it to a muffle furnace and pre-sinter it at a temperature of 800°C for 4 h. Cool it to room temperature with the furnace and then perform a second ball milling until the powder particle size is 10 μm. Then, press the mixed powder into a shape at a pressure of 20 MPa. Finally, sinter it at 1300°C for 5 h and cool it naturally to obtain manganese-zinc ferrite.

[0036] (4) Add 10 parts by weight of ferrocene-based polymer magnet, 100 parts by weight of manganese-zinc ferrite and 3 parts by weight of polyethylene wax into a high-speed mixer, mix them evenly at a speed of 8000 r / min, and then press them at 200 MPa to obtain a doped manganese-zinc ferrite core.

[0037] Example 3

[0038] (1) Add 100 parts by weight of 1,1′-ferrocenedicarboxylic acid, 85 parts by weight of thionyl chloride and 2 parts by weight of N,N-dimethylformamide into a reaction flask, react at 100° C. for 3 h, and distill under reduced pressure to obtain 1,1′-ferrocenedicarboxylic acid chloride.

[0039] (2) Add 100 parts by weight of 1,1′-ferrocene dicarbonyl chloride and N,N-dimethylacetamide solvent to a reaction flask, stir evenly, then add 50 parts of [2,2′-bipyridine]-5,5′-diamine and 75 parts of triethylamine, stir and react, first at 10°C for 1 hour and then at 35°C for 4 hours, then add methanol to precipitate, filter, wash with deionized water until neutral, and dry to obtain a ferrocene-based polymer magnet.

[0040] (3) 65 parts by weight of iron oxide, 20 parts by weight of manganese oxide, 15 parts by weight of zinc oxide, 0.05 parts by weight of lanthanum oxide and 0.1 parts by weight of grain boundary strengthener Al2O3 were added to a ball mill and ball-milled at a speed of 200 r / min for 16 h. The mixture was then added to a muffle furnace and pre-fired at 1000°C for 2 h. The mixture was cooled to room temperature with the furnace and then ball-milled for a second time until the powder particle size was 5 μm. The mixed powder was then pressed into a mold at a pressure of 15 MPa and finally sintered at 1450°C for 3 h. The mixture was naturally cooled to obtain manganese-zinc ferrite.

[0041] (4) 15 parts by weight of ferrocene-based polymer magnet, 100 parts by weight of manganese-zinc ferrite and 0.5 parts by weight of polyethylene wax were added into a high-speed mixer, mixed evenly at a speed of 5000 r / min, and then pressed at 300 MPa to obtain a doped manganese-zinc ferrite core.

[0042] Example 4

[0043] (1) Add 30 parts by weight of 1,1′-ferrocenedicarboxylic acid, 33 parts by weight of thionyl chloride and 1.2 parts by weight of N,N-dimethylformamide into a reaction flask, react at 85°C for 7 hours, and distill under reduced pressure to obtain 1,1′-ferrocenedicarboxylic acid chloride.

[0044] (2) Add 20 parts by weight of 1,1′-ferrocene dicarbonyl chloride and N,N-dimethylacetamide solvent to a reaction flask, stir evenly, then add 13 parts of [2,2′-bipyridine]-5,5′-diamine and 17 parts of triethylamine, stir and react, first at 8°C for 2.5 h and then at 30°C for 5.5 h, then add methanol to precipitate, filter, wash with deionized water until neutral, and dry to obtain a ferrocene-based polymer magnet.

[0045] (3) 58 parts by weight of iron oxide, 32 parts of manganese oxide, 10 parts of zinc oxide, 0.08 parts of lanthanum oxide and 0.1 parts of grain boundary strengthener CaCO3 were added to a ball mill and ball-milled at a speed of 260 r / min for 13 h. The mixture was then added to a muffle furnace and pre-fired at 950°C for 3 h. The mixture was cooled to room temperature with the furnace and then ball-milled for a second time until the powder particle size was 6 μm. The mixed powder was then pressed into a mold at a pressure of 17 MPa and finally sintered at 1350°C for 4 h. The mixture was naturally cooled to obtain manganese-zinc ferrite.

[0046] (4) 20 parts by weight of ferrocene-based polymer magnet, 100 parts by weight of manganese-zinc ferrite and 2.5 parts by weight of polyethylene wax were added into a high-speed mixer, mixed evenly at a speed of 6500 r / min, and then pressed at 220 MPa to obtain a doped manganese-zinc ferrite core.

[0047] Example 5

[0048] (1) Add 80 parts by weight of 1,1′-ferrocenedicarboxylic acid, 72 parts by weight of thionyl chloride and 2.8 parts by weight of N,N-dimethylformamide into a reaction flask, react at 95°C for 6 hours, and distill under reduced pressure to obtain 1,1′-ferrocenedicarboxylic acid chloride.

[0049] (2) Add 40 parts by weight of 1,1′-ferrocene dicarbonyl chloride and N,N-dimethylacetamide solvent to a reaction flask, stir evenly, then add 22 parts of [2,2′-bipyridine]-5,5′-diamine and 34 parts of triethylamine, stir and react, first at 4°C for 3 h and then at 20°C for 8 h, then add methanol to precipitate, filter, wash with deionized water until neutral, and dry to obtain a ferrocene-based polymer magnet.

[0050] (3) 61 parts of iron oxide, 25 parts of manganese oxide, 14 parts of zinc oxide, 0.1 parts of lanthanum oxide and 0.1 parts of grain boundary strengthener SiO2 in proportions by weight were added to a ball mill and ball-milled at a speed of 290 r / min for 16 h. The mixture was then added to a muffle furnace and pre-fired at 850°C for 3 h. The mixture was cooled to room temperature with the furnace and ball-milled for a second time until the powder particle size was 7 μm. The mixed powder was then pressed into a shape at a pressure of 16 MPa and sintered at 1300°C for 5 h. The mixture was naturally cooled to obtain manganese-zinc ferrite.

[0051] (4) 25 parts by weight of ferrocene-based polymer magnet, 100 parts by weight of manganese-zinc ferrite and 3 parts by weight of polyethylene wax were added into a high-speed mixer, mixed evenly at a speed of 8000 r / min, and then pressed at 210 MPa to obtain a doped manganese-zinc ferrite core.

[0052] Comparative Example 1

[0053] 100 parts by weight of manganese-zinc ferrite and 2 parts of polyethylene wax were added into a high-speed mixer, mixed evenly at a rotation speed of 7500 r / min, and then pressed at 260 MPa to obtain a manganese-zinc ferrite core.

[0054] Comparative Example 2

[0055] (1) 60 parts by weight of iron oxide, 30 parts by weight of manganese oxide, 10 parts by weight of zinc oxide and 0.1 parts by weight of grain boundary strengthener CaCO3 were added to a ball mill and milled at a speed of 250 r / min for 12 h. The mixture was then added to a muffle furnace and pre-fired at 900°C for 3 h. The mixture was cooled to room temperature with the furnace and then ball-milled for a second time until the powder particle size was 8 μm. The mixed powder was then pressed into a mold at a pressure of 18 MPa and finally sintered at 1400°C for 4 h. The mixture was naturally cooled to obtain manganese-zinc ferrite.

[0056] (2) Add 5 parts by weight of ferrocene-based polymer magnet, 100 parts by weight of manganese-zinc ferrite and 2 parts by weight of polyethylene wax into a high-speed mixer, mix them evenly at a speed of 7500 r / min, and then press them at 260 MPa to obtain a manganese-zinc ferrite core.

[0057] Magnetic property test: The magnetic properties of the prepared manganese-zinc ferrite core were tested using a vibrating sample magnetometer.

[0058] Saturation magnetization (emu / g) Coercivity (Oe) Saturation flux density (mT) Example 1 78.90 107.32 490.3 Example 2 80.84 111.78 499.8 Example 3 83.18 116.24 512.4 Example 4 87.32 115.55 545.3 Example 5 88.67 114.82 548.7 Comparative Example 1 56.20 105.52 450.3 Comparative Example 2 60.36 108.36 462.1

[0059] The saturation magnetization intensity is the maximum magnetization intensity that can be achieved when magnetized in an external magnetic field. The higher the saturation magnetization intensity, the better. From the test results in the above table, it can be seen that with the increase of the content of ferrocene-based polymer magnet and rare earth lanthanum in the doped manganese-zinc ferrite core material, the saturation magnetization intensity of the core material continues to increase, reaching the maximum in Example 5, which is 88.67emu / g. This is because the appropriate amount of La 3+ Enter the octahedral structure of MnZn ferrite to replace Fe 3+ , La 3+ The radius is much larger than Fe 3+ radius, so La 3+ Replace Fe 3+ After that, the excess rare earth La is adsorbed around the ferrite grain boundary, exerting a certain pressure on the grain boundary, thereby improving the saturation magnetization intensity of the material. At the same time, the addition of ferrocene polymer magnet enhances the magnetic properties of the core. This is because the charge of the iron ions in ferrocene is transferred to generate a mixed valence of divalent iron and trivalent iron, and the bipyridine structure on the polymer chain can form coordination with the iron ions and lanthanum ions in the manganese-zinc ferrite, promoting the close combination of the two, so that the magnetic properties of the composite core are greatly improved.

[0060] Coercive force is the reverse magnetic field strength that must be applied to reduce the magnetic induction intensity of a magnet after it has been magnetized to zero; as the doping amount increases, heterogeneous impurities are enriched at the grain boundaries, causing the coercive force to increase, but the overall change is not significant, indicating that the prepared core material is easily magnetized by an external magnetic field and easily demagnetized by an applied magnetic field or other factors, resulting in low magnetic loss, which makes up for the limitations of conventional ferrite cores in certain high-frequency and microwave frequency band applications.

[0061] The greater the saturation flux density, the more obvious the core effect is, and it is not easy to deform. It can be seen from the test results in the above table that with the increase of the doping amount, the saturation flux density of the core is enhanced, reaching a maximum of 548.7mT. The magnetic permeability of the core prepared in this way is high, and the high saturation flux density of the material is achieved, while maintaining the material's higher initial permeability and lower power consumption; while Comparative Example 1 is only 450.3mT, and Comparative Example 2 is only 462.1mT, and the saturation flux density is lower. This is because the comparative examples are not doped with ferrocene-based polymer magnets and rare earth lanthanum, resulting in poor magnetic properties.

[0062] Example 6

[0063] (1) 60 parts by weight of iron oxide, 30 parts by weight of manganese oxide, 10 parts by weight of zinc oxide, 0.01 parts by weight of lanthanum oxide and 0.2 parts by weight of grain boundary strengthener CaCO3 were added to a ball mill and ball-milled at a speed of 250 r / min for 12 h. The mixture was then added to a muffle furnace and pre-fired at 900°C for 3 h. The mixture was cooled to room temperature with the furnace and ball-milled for a second time until the powder particle size was 8 μm. The mixed powder was then pressed into a mold at a pressure of 18 MPa and finally sintered at 1400°C for 4 h. The mixture was naturally cooled to obtain manganese-zinc ferrite.

[0064] (2) Add 5 parts by weight of ferrocene-based polymer magnet, 100 parts by weight of manganese-zinc ferrite and 2 parts by weight of polyethylene wax into a high-speed mixer, mix them evenly at a speed of 7500 r / min, and then press them at 260 MPa to obtain a doped manganese-zinc ferrite core.

[0065] Example 7

[0066] (1) 60 parts by weight of iron oxide, 30 parts by weight of manganese oxide, 10 parts by weight of zinc oxide, 0.01 parts by weight of lanthanum oxide and 0.3 parts by weight of grain boundary strengthener CaCO3 were added to a ball mill and milled once at a speed of 250 r / min for 12 h. The mixture was then added to a muffle furnace and pre-fired at 900°C for 3 h. The mixture was cooled to room temperature with the furnace and then ball-milled for a second time until the powder particle size was 8 μm. The mixed powder was then pressed into a mold at a pressure of 18 MPa and finally sintered at 1400°C for 4 h. The mixture was naturally cooled to obtain manganese-zinc ferrite.

[0067] (2) Add 5 parts by weight of ferrocene-based polymer magnet, 100 parts by weight of manganese-zinc ferrite and 2 parts by weight of polyethylene wax into a high-speed mixer, mix them evenly at a speed of 7500 r / min, and then press them at 260 MPa to obtain a doped manganese-zinc ferrite core.

[0068] Example 8

[0069] (1) 60 parts by weight of iron oxide, 30 parts by weight of manganese oxide, 10 parts by weight of zinc oxide, 0.01 parts by weight of lanthanum oxide and 0.4 parts by weight of grain boundary strengthener CaCO3 were added to a ball mill and milled once at a speed of 250 r / min for 12 h. The mixture was then added to a muffle furnace and pre-fired at 900°C for 3 h. The mixture was cooled to room temperature with the furnace and then ball-milled for a second time until the powder particle size was 8 μm. The mixed powder was then pressed into a shape at a pressure of 18 MPa and finally sintered at 1400°C for 4 h. The mixture was naturally cooled to obtain manganese-zinc ferrite.

[0070] (2) Add 5 parts by weight of ferrocene-based polymer magnet, 100 parts by weight of manganese-zinc ferrite and 2 parts by weight of polyethylene wax into a high-speed mixer, mix them evenly at a speed of 7500 r / min, and then press them at 260 MPa to obtain a doped manganese-zinc ferrite core.

[0071] Example 9

[0072] (1) 60 parts by weight of iron oxide, 30 parts by weight of manganese oxide, 10 parts by weight of zinc oxide, 0.01 parts by weight of lanthanum oxide and 0.5 parts by weight of grain boundary strengthener CaCO3 were added to a ball mill and milled at a speed of 250 r / min for 12 h. The mixture was then added to a muffle furnace and pre-fired at 900°C for 3 h. The mixture was cooled to room temperature with the furnace and then ball-milled for a second time until the powder particle size was 8 μm. The mixed powder was then pressed into a mold at a pressure of 18 MPa and finally sintered at 1400°C for 4 h. The mixture was naturally cooled to obtain manganese-zinc ferrite.

[0073] (2) Add 5 parts by weight of ferrocene-based polymer magnet, 100 parts by weight of manganese-zinc ferrite and 2 parts by weight of polyethylene wax into a high-speed mixer, mix them evenly at a speed of 7500 r / min, and then press them at 260 MPa to obtain a doped manganese-zinc ferrite core.

[0074] Comparative Example 3

[0075] (1) Add 60 parts of iron oxide, 30 parts of manganese oxide, 10 parts of zinc oxide and 0.01 parts of lanthanum oxide by weight into a ball mill, and perform a ball milling at a rotation speed of 250 r / min for 12 h. Then add it to a muffle furnace and pre-sinter it at a temperature of 900°C for 3 h. Cool it to room temperature with the furnace, and then perform a second ball milling until the powder particle size is 8 μm. Then, press the mixed powder into a shape at a pressure of 18 MPa, and finally sinter it at 1400°C for 4 h. Then, cool it naturally to obtain manganese-zinc ferrite.

[0076] (2) Add 5 parts by weight of ferrocene-based polymer magnet, 100 parts by weight of manganese-zinc ferrite and 2 parts by weight of polyethylene wax into a high-speed mixer, mix them evenly at a speed of 7500 r / min, and then press them at 260 MPa to obtain a manganese-zinc ferrite core.

[0077] Power loss test: The power loss of samples at 25°C, 60°C and 100°C were measured using a BH analyzer at 500kHz and 50mT.

[0078]

[0079] When the frequency of the transmitted electromagnetic wave is constant, the higher the operating temperature, the greater the power loss of the magnetic device made of ferrite. It can be seen from the test results in the above table that in the embodiment, with the increase of the content of the grain boundary strengthener, the power loss is significantly reduced. This is because the grain boundary strengtheners CaCO3, SiO2, and Al2O3 can reduce the power loss of the sample. During the sintering process of preparing manganese-zinc ferrite, CaCO3 and SiO2 will generate high-resistivity CaSiO3, which accumulates at high concentrations at the grain boundaries, thereby increasing the grain boundary resistivity. During the high-temperature sintering process, Al2O3 can generate a layer of low-conductivity protective film on the surface of the ferrite to form a shell-core structure, thereby increasing the resistivity inside the ferrite grains. The increase in the resistivity of the grain boundaries and grains effectively reduces the power loss of the material.

[0080] Comparative Example 1 does not contain ferrocene-based polymer magnets, and its power loss at 25°C is 85.12 mW / cm 3 , which is significantly higher than that of the embodiment. This is because the ferrocene-based polymer magnet has a small magnetic loss on the transmission signal in a wide range of electromagnetic wave frequencies, and its electromagnetic performance is very stable in a wide temperature range, which makes its power loss value small; Comparative Example 2 does not contain rare earth lanthanum, and its power loss at 100°C is 158.59mW / cm 3 , the loss is large; Comparative Example 3 does not contain a grain boundary strengthener, and its power loss at 60°C is 102.23mW / cm 3 , the loss is more obvious.

[0081] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and the implementation modes. They can be fully applied to various fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the claims and the scope of equivalents, the present invention is not limited to the specific details and the embodiments shown and described herein.

Claims

1. A method for preparing a magnetic core, for preparing a doped manganese-zinc ferrite magnetic core, characterized in that: The doped manganese-zinc ferrite core comprises the following components in parts by weight: 5-25 parts of ferrocene-based polymer magnet, 100 parts of manganese-zinc ferrite and 0.5-3 parts of polyethylene wax; The preparation method comprises: adding the above-mentioned proportion of ferrocene-based polymer magnet, manganese zinc ferrite and polyethylene wax into a high-speed mixer, mixing them evenly at a rotation speed of 5000-8000 r / min, and then pressing and molding them at 200-300 MPa to obtain a doped manganese zinc ferrite core; The preparation method of the manganese-zinc ferrite is as follows: 55-65 parts of iron oxide, 20-35 parts of manganese oxide, 5-15 parts of zinc oxide, 0.01-0.1 parts of lanthanum oxide and 0.1-0.5 parts of grain boundary strengthener are added into a ball mill by weight, and ball milled for 8-16 hours at a rotation speed of 200-300 r / min, and then added into a muffle furnace, and pre-sintered for 2-4 hours at a temperature of 800-1000° C., cooled to room temperature with the furnace, and then ball milled for a second time until the powder particle size is 5-10 μm, and then the mixed powder is pressed into shape, and finally sintered at 1300-1450° C. for 3-5 hours, and cooled naturally to obtain the manganese-zinc ferrite; The preparation method of the ferrocene-based polymer magnet is as follows: (1) Add 100 parts by weight of 1,1′-ferrocenedicarboxylic acid, 85-110 parts by weight of thionyl chloride and 2-5 parts by weight of N,N-dimethylformamide into a reaction flask, stir to react, and after the reaction is completed, perform vacuum distillation to obtain 1,1′-ferrocenedicarboxylic acid chloride; (2) Add 1,1′-ferrocene dicarbonyl chloride and N,N-dimethylacetamide solvent to the reaction flask, stir evenly, then add [2,2′-bipyridine]-5,5′-diamine and triethylamine, stir and react. After the reaction is completed, add methanol to precipitate, filter, wash with deionized water until neutral, and dry to obtain a ferrocene-based polymer magnet; In the step (2), by weight, 1,1′-ferrocenyl dicarbonyl chloride is 100 parts, [2,2′-bipyridine]-5,5′-diamine is 50-70 parts, and triethylamine is 75-90 parts; The reaction in step (2) is first carried out at 0-10°C for 1-4 hours, and then at 20-35°C for 4-8 hours.

2. The method for preparing a magnetic core according to claim 1, characterized in that: The grain boundary strengthener is any one of CaCO3, SiO2, and Al2O3.

3. The method for preparing a magnetic core according to claim 1, characterized in that: The pressure of the compression molding is 15-20 MPa.

4. The method for preparing a magnetic core according to claim 1, characterized in that: In the step (1), the reaction temperature is 80-100° C. and the reaction time is 3-8 h.

Citation Information

Patent Citations

  • Preparation method of high-performance manganese-zinc MnZn soft magnetic ferrite material

    CN102992750A

  • Manganese-based ferrite core material used for transformer

    CN104051112A