A water-soluble temporary plugging agent for acid fracturing of oil and water wells and its production process
Through the combination of starch cross-linked carboxymethyl cellulose and amino acid-acrylamide polymer and fiber diversity design, a high temperature resistant, degradable water-soluble temporary plugging agent for acidification fracturing of oil and water wells is prepared, which solves the problem of traditional temporary plugging. The deficiencies of the agent in low-permeability oil fields and high-temperature conditions improve oil well recovery and acidification fluid utilization efficiency.
Patent Information
- Application Number
- CN202410936600.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-07-12
AI Technical Summary
Traditional gel particle temporary plugging agents have low underground cross-linking strength and weak gel-forming ability. They cannot effectively solve the formation complexity and high-temperature plugging problems in low-permeability tight oil fields, resulting in a decrease in oil well productivity.
Starch cross-linked carboxymethylcellulose is mixed with amino acid-acrylamide polymer, and a water-soluble temporary plugging agent for acidification fracturing of oil and water wells is prepared through microwave cross-linking and coaxial spinning technology, combining various shapes and granular structures of fibers. , enhance its thermal stability and water absorption capacity, and form a temporary plugging agent suitable for high temperature environments.
The water-soluble temporary plugging agent for acid fracturing of oil and water wells is degradable, has high water absorption and high temperature resistance, effectively prevents acidizing fluid from entering the high permeability zone, improves the utilization rate of acidifying fluid, and blocks gaps through fiber bridges to promote fracture diversion. , improve oil well recovery.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of petrochemical industry, in particular to a water-soluble temporary plugging agent for acid fracturing of oil and water wells and a production process thereof. Background Art
[0002] With the continuous improvement of the exploration and development of oil and gas resources, the exploration field is gradually moving towards complex high-temperature formations such as deep and ultra-deep layers on land, deep-water layers in the ocean, high-temperature geothermal and hot dry rocks. Generally, the temperature of a well with a depth of 2000 to 3000 meters is between 60 and 80 ℃ Mostly , over 150℃ is defined as high temperature formation, and the temperature of some high temperature formations even exceeds 200℃. And with the extension of mining time, the formation conditions of oil wells are becoming more and more complicated, and the requirements for temporary plugging agents are getting higher and higher. Temporary plugging agents are required to have high action accuracy, wide action range, strong comprehensive performance and other important characteristics.
[0003] Acidizing treatment is a common measure to remove formation damage and restore reservoir permeability. It mainly injects acidizing fluid into the formation to dissolve clay particles, carbonates, etc., thereby dredging the flow channel of the fluid and increasing the permeability of the near-well zone, so as to achieve the purpose of improving and increasing the oil well yield. However, in the conventional acidizing process, the acidizing fluid often enters the high permeability zone along the channel with low resistance, and the acid cannot be evenly distributed. In this case, the reservoir needs to be stratified. At present, the stratified acidizing process mainly includes mechanical stratification and chemical stratification. Traditional mechanical stratified acidizing is not only costly, time-consuming, and the construction process is limited. In addition, factors such as well condition deterioration also increase the construction risk to a certain extent; and the low permeability fractured sandstone reservoir has a complex structure, uneven distribution, strong stress sensitivity, serious vertical heterogeneity, a large range of dynamic width, and is easily damaged. There is often a blocking phenomenon in the process. Therefore, it is necessary to carry out fracturing construction in low permeability and tight oil fields. The fractured formation begins to produce oil slowly. As the oilfield is developed, the formation pore pressure gradually decreases, the proppant breaks, the fractures begin to close, and the recovery of raw materials decreases. Therefore, in order to increase the recovery rate and improve economic benefits, it is necessary to use temporary plugging agents to temporarily plug the reservoir and turn it into fracturing. However, the traditional gel particle temporary plugging agent has low cross-linking strength and weak gelling ability underground. Therefore, it is particularly necessary to invent a water-soluble temporary plugging agent for acid fracturing of oil and water wells. Summary of the invention
[0004] The purpose of the present invention is to provide a water-soluble temporary plugging agent for acid fracturing of oil and water wells and a production process thereof, so as to solve the problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: a water-soluble temporary plugging agent for acid fracturing of oil and water wells, wherein the water-soluble temporary plugging agent for acid fracturing of oil and water wells is prepared by mixing starch cross-linked carboxymethyl cellulose with an amino acid-acrylamide polymer, and the mixture is made into particles and fibers through a process.
[0006] Furthermore, the fibers are specifically hollow long and thin fibers, hollow short and thin fibers, hollow thick and long fibers, and hollow thick and short fibers.
[0007] Furthermore, a method for preparing a water-soluble temporary plugging agent for acid fracturing of oil and water wells comprises the following preparation steps:
[0008] (1) Carboxymethyl cellulose and deionized water are mixed, stirred at 25-35°C and 80-130 rpm for 20-60 min, potato starch aqueous solution, sodium trimetaphosphate and anhydrous sodium sulfate are added, nitrogen is introduced at 10 mL / min, microwave cross-linking is performed at a power of 280-420 W for 5-15 min, then immersed in methanol for 4 h, dried at 50-80°C for 10-16 h, crushed and passed through an 80-mesh sieve to obtain starch-cross-linked carboxymethyl cellulose; the potato starch aqueous solution contains 40% by weight of potato starch;
[0009] (2) Mix polyacrylamide, amino acid and deionized water, heat to 60°C, stir at 60-100 rpm for 50-80 min, add potassium persulfate, sodium diisobutylnaphthalene sulfonate, urea and starch cross-linked carboxymethyl cellulose, heat to 60-90°C, react for 4-10 h to obtain a copolymer;
[0010] (3) The copolymer was heated to 70-100°C and air was used as the core for coaxial spinning. The parameters were as follows: the inner needle diameter was 0.56 mm, the outer needle diameters were 2.01 mm and 4.21 mm, respectively, the receiving distance was 20 cm, and the feed rate was 20-50 mL / h, to obtain hollow coarse fibers and hollow fine fibers. Subsequently, hollow fine long fibers, hollow fine short fibers, hollow coarse long fibers, and hollow coarse short fibers were obtained by shearing, respectively.
[0011] (4) The copolymer is ground and passed through a 20-200 mesh sieve to obtain particles, which are then mixed with hollow long and thin fibers, hollow short and thin fibers, hollow thick and long fibers, and hollow thick and short fibers to obtain a water-soluble temporary plugging agent for acid fracturing of oil and water wells.
[0012] Furthermore, in step (1), the mass ratio of the carboxymethyl cellulose, deionized water, potato starch aqueous solution, sodium trimetaphosphate, and anhydrous sodium sulfate is 0.1-0.8:3-5:2:1.2-2:1.
[0013] Furthermore, the molecular weight of the polyacrylamide in step (2) is 2×10 6 .
[0014] Furthermore, in step (2), the mass ratio of polyacrylamide, amino acid, deionized water, potassium persulfate, sodium diisobutylnaphthalene sulfonate, urea, and starch-cross-linked carboxymethyl cellulose is 5:5:10~30:0.5:0.01:0.9:0.9~1.8.
[0015] Furthermore, in step (3), the length of the long fibers is 10 mm, and the length of the short fibers is 1 mm.
[0016] Furthermore, in step (4), the mass ratio of the particles, the hollow long and thin fibers, the hollow short and thin fibers, the hollow thick and long fibers, and the hollow thick and short fibers is 0.9-3:1:1:1:1.
[0017] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0018] The water-soluble temporary plugging agent of the present invention is prepared by mixing starch-crosslinked carboxymethyl cellulose with an amino acid-acrylamide polymer, and is made into particles and fibers through a process and mixed to achieve the effects of being degradable, having a high water absorption rate and being resistant to high temperatures.
[0019] Firstly, starch and carboxymethyl cellulose are irradiated and cross-linked with the assistance of sodium trimetaphosphate. The active reaction points on the surface of cellulose are stimulated by microwaves, so that the carboxymethyl groups penetrate or break from the surface of starch particles from the outside to the inside. At the same time, covalent bonds with stronger force than hydrogen bonds are introduced through this cross-linking reaction, and the molecules are connected in the form of bridges to form a network structure, thereby improving the thermal stability of starch and the water absorption rate of the matrix. Then, a scaffolding effect is provided in the amino acid-acrylamide interpenetrating structure to form a copolymer with a certain spatial network structure, so that it has appropriate solubility at high temperature.
[0020] Secondly, using air as the core layer, hollow fine fibers and hollow coarse fibers are made by coaxial spinning, making them easier to fit and fill uneven cracks or wormholes, thereby increasing their own specific surface area and enhancing their water absorption capacity, thereby hindering the acidizing fluid from entering the high permeability area, playing the role of diverting the acidizing fluid, prompting the main acidizing fluid to be diverted and injected into the low permeability area, and improving the effective utilization rate of the acidizing fluid. At the same time, through shearing, hollow fine fibers and hollow coarse fibers of different lengths are made to avoid mutual entanglement due to aggregation, and the copolymer is made into granules, which has a certain compaction effect on the fiber and promotes the sedimentation of the fiber. Under the action of pressure difference, the coarse and short fibers first form bridges at the pore throats, increasing the flow resistance and reducing the flow rate. The fine fibers and particles begin to settle in the pores and continue to move to the deep formation to further fill the bridge gaps, gradually forming a temporary plugging zone with extremely poor permeability, thereby causing a change in the stress field around the temporary plugging layer, realizing a local environment that is conducive to crack diversion, and achieving the purpose of assisting repeated fracturing crack diversion. DETAILED DESCRIPTION
[0021] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0022] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of the water-soluble temporary plugging agent for acid fracturing of oil and water wells prepared in the following examples are as follows:
[0023] Water absorption: Take the embodiment and comparative example of the same size, put them in deionized water at 80°C, let them stand for 180 minutes, then take them out and test their expansion multiples.
[0024] High temperature resistance: Take the embodiment and comparative example of the same size, put them in deionized water at 100°C, let them stand for 10 hours, then take them out and test their solubility.
[0025] Degradation: Take the example and the comparative example of the same size, place them in deionized water at 80°C, let them stand for 24 hours, and record their dissolution state.
[0026] Example 1
[0027] (1) Carboxymethyl cellulose and deionized water are mixed, stirred at 25°C and 80 rpm for 20 min, potato starch aqueous solution, sodium trimetaphosphate and anhydrous sodium sulfate are added, nitrogen is introduced at 10 mL / min, microwave cross-linking is performed at a power of 280 W for 5 min, then the mixture is immersed in methanol for 4 h, dried at 50°C for 10 h, and crushed through an 80-mesh sieve to obtain starch-cross-linked carboxymethyl cellulose; the mass ratio of the carboxymethyl cellulose, deionized water, potato starch aqueous solution, sodium trimetaphosphate and anhydrous sodium sulfate is 0.1:3:2:1.2:1; the weight fraction of potato starch in the potato starch aqueous solution is 40%;
[0028] (2) The molecular weight is 2×10 6 The polyacrylamide, amino acid and deionized water were mixed, heated to 60°C, stirred at 60rpm for 50min, potassium persulfate, sodium diisobutylnaphthalenesulfonate, urea and starch cross-linked carboxymethyl cellulose were added, heated to 60°C, reacted for 4h, and a copolymer was obtained; the molecular weight was 2×10 6 The mass ratio of polyacrylamide, amino acid, deionized water, potassium persulfate, sodium diisobutylnaphthalene sulfonate, urea, and starch cross-linked carboxymethyl cellulose is 5:5:10:0.5:0.01:0.9:0.9;
[0029] (3) The copolymer was heated to 70°C and air was used as the core for coaxial spinning. The parameters were as follows: inner needle diameter was 0.56 mm, outer needle diameters were 2.01 mm and 4.21 mm, respectively, receiving distance was 20 cm, and feed rate was 20 mL / h. Hollow coarse fibers and hollow thin fibers were obtained. Subsequently, hollow thin long fibers and hollow coarse long fibers with a length of 10 mm, hollow thin short fibers and hollow coarse short fibers with a length of 1 mm were obtained by shearing, respectively.
[0030] (4) Grinding the copolymer and passing it through a 20-mesh sieve to obtain particles, which are then mixed with hollow long and thin fibers, hollow short and thin fibers, hollow thick and long fibers, and hollow short and thin fibers to obtain a water-soluble temporary plugging agent for acid fracturing of oil and water wells; the mass ratio of the particles, hollow long and thin fibers, hollow short and thin fibers, hollow thick and long fibers, and hollow short and thin fibers is 0.9:1:1:1:1.
[0031] Example 2
[0032] (1) Carboxymethyl cellulose and deionized water are mixed, stirred at 30°C and 100 rpm for 45 min, potato starch aqueous solution, sodium trimetaphosphate and anhydrous sodium sulfate are added, nitrogen is introduced at 10 mL / min, microwave cross-linking is performed at a power of 360 W for 8 min, then the mixture is immersed in methanol for 4 h, dried at 70°C for 13 h, and crushed through an 80-mesh sieve to obtain starch-cross-linked carboxymethyl cellulose; the mass ratio of the carboxymethyl cellulose, deionized water, potato starch aqueous solution, sodium trimetaphosphate and anhydrous sodium sulfate is 0.5:4:2:1.5:1; the weight fraction of potato starch in the potato starch aqueous solution is 40%;
[0033] (2) The molecular weight is 2×10 6 The polyacrylamide, amino acid and deionized water were mixed, heated to 60°C, stirred at 80rpm for 60min, potassium persulfate, sodium diisobutylnaphthalenesulfonate, urea and starch cross-linked carboxymethyl cellulose were added, heated to 75°C, reacted for 7h, and a copolymer was obtained; the molecular weight was 2×10 6 The mass ratio of polyacrylamide, amino acid, deionized water, potassium persulfate, sodium diisobutylnaphthalene sulfonate, urea, and starch cross-linked carboxymethyl cellulose is 5:5:20:0.5:0.01:0.9:1.5;
[0034] (3) The copolymer was heated to 85°C and air was used as the core for coaxial spinning. The parameters were as follows: the inner needle diameter was 0.56 mm, the outer needle diameters were 2.01 mm and 4.21 mm, respectively, the receiving distance was 20 cm, and the feed rate was 20-50 mL / h. Hollow coarse fibers and hollow thin fibers were obtained. Subsequently, hollow thin long fibers and hollow coarse long fibers with a length of 10 mm, hollow thin short fibers and hollow coarse short fibers with a length of 1 mm were obtained by shearing, respectively.
[0035] (4) Grinding the copolymer and passing it through a 110-mesh sieve to obtain granules, which are then mixed with hollow long and thin fibers, hollow short and thin fibers, hollow thick and long fibers, and hollow short and thin fibers to obtain a water-soluble temporary plugging agent for acid fracturing of oil and water wells; the mass ratio of the granules, hollow long and thin fibers, hollow short and thin fibers, hollow thick and long fibers, and hollow short and thin fibers is 2:1:1:1:1.
[0036] Example 3
[0037] (1) Carboxymethyl cellulose and deionized water are mixed, stirred at 35° C. and 130 rpm for 60 min, potato starch aqueous solution, sodium trimetaphosphate and anhydrous sodium sulfate are added, nitrogen is introduced at 10 mL / min, microwave cross-linking is performed at a power of 420 W for 15 min, then the mixture is immersed in methanol for 4 h, dried at 80° C. for 16 h, and crushed through an 80-mesh sieve to obtain starch-cross-linked carboxymethyl cellulose; the mass ratio of the carboxymethyl cellulose, deionized water, potato starch aqueous solution, sodium trimetaphosphate and anhydrous sodium sulfate is 0.8:5:2:2:1; the weight fraction of potato starch in the potato starch aqueous solution is 40%;
[0038] (2) The molecular weight is 2×10 6 The polyacrylamide, amino acid and deionized water were mixed, heated to 60°C, stirred at 100 rpm for 80 min, potassium persulfate, sodium diisobutylnaphthalene sulfonate, urea and starch cross-linked carboxymethyl cellulose were added, heated to 90°C, reacted for 10 h, and a copolymer was obtained; the molecular weight was 2×10 6 The mass ratio of polyacrylamide, amino acid, deionized water, potassium persulfate, sodium diisobutylnaphthalene sulfonate, urea, and starch cross-linked carboxymethyl cellulose is 5:5:30:0.5:0.01:0.9:1.8;
[0039] (3) The copolymer was heated to 100°C and air was used as the core for coaxial spinning. The parameters were as follows: the inner needle diameter was 0.56 mm, the outer needle diameters were 2.01 mm and 4.21 mm, respectively, the receiving distance was 20 cm, and the feed rate was 50 mL / h. Hollow coarse fibers and hollow thin fibers were obtained. Subsequently, hollow thin long fibers and hollow coarse long fibers with a length of 10 mm, hollow thin short fibers and hollow coarse short fibers with a length of 1 mm were obtained by shearing, respectively.
[0040] (4) Grinding the copolymer and passing it through a 200-mesh sieve to obtain particles, which are then mixed with hollow long and thin fibers, hollow short and thin fibers, hollow thick and long fibers, and hollow short and thin fibers to obtain a water-soluble temporary plugging agent for acid fracturing of oil and water wells; the mass ratio of the particles, hollow long and thin fibers, hollow short and thin fibers, hollow thick and long fibers, and hollow short and thin fibers is 3:1:1:1:1.
[0041] Comparative Example 1
[0042] The difference between Comparative Example 1 and Example 2 is that step (1) is different. Step (1) is changed to: carboxymethyl cellulose and deionized water are mixed, stirred at 30° C. and 100 rpm for 45 min, potato starch aqueous solution, sodium trimetaphosphate and anhydrous sodium sulfate are added, nitrogen is introduced at 10 mL / min, the temperature is raised to 65° C., the reaction is carried out for 10 h, and then the mixture is immersed in methanol for 4 h, dried at 70° C. for 13 h, and crushed through an 80-mesh sieve to obtain starch cross-linked carboxymethyl cellulose; the mass ratio of the carboxymethyl cellulose, deionized water, potato starch aqueous solution, sodium trimetaphosphate and anhydrous sodium sulfate is 0.5:4:2:1.5:1; the weight fraction of potato starch in the potato starch aqueous solution is 40%; and the remaining steps are the same as those in Example 2.
[0043] Comparative Example 2
[0044] The difference between Comparative Example 2 and Example 2 is that step (3) is different. Step (3) is changed to: the copolymer is heated to 85°C and spun with the following parameters: needle diameters are 2.01 mm and 4.21 mm, respectively, the receiving distance is 20 cm, and the feed rate is 20-50 mL / h to obtain coarse fibers and fine fibers. Subsequently, by shearing, thin and long fibers and coarse and long fibers with a length of 10 mm, and thin and short fibers and coarse and short fibers with a length of 1 mm are obtained respectively. The remaining steps are the same as those in Example 2.
[0045] Comparative Example 3
[0046] The difference between Comparative Example 3 and Example 2 is that step (3) is different. Step (3) is changed to: the copolymer is heated to 85°C, air is used as the core, and coaxial spinning is carried out. Its parameters are: inner needle diameter is 0.56 mm, outer needle diameter is 2.01 mm, receiving distance is 20 cm, and feed rate is 20~50 mL / h, to obtain hollow fibers, and then, by shearing, hollow long fibers with a length of 10 mm and hollow short fibers with a length of 1 mm are obtained respectively; the remaining steps are the same as Example 2.
[0047] Comparative Example 4
[0048] The difference between Comparative Example 4 and Example 2 is that step (3) is different. Step (3) is changed to: the copolymer is heated to 85°C, air is used as the core, and coaxial spinning is carried out. Its parameters are: inner needle diameter is 0.56 mm, outer needle diameter is 4.21 mm, receiving distance is 20 cm, and feed rate is 20~50 mL / h, to obtain hollow fibers, and then, by shearing, hollow long fibers with a length of 10 mm and hollow short fibers with a length of 1 mm are obtained respectively; the remaining steps are the same as Example 2.
[0049] Comparative Example 5
[0050] The difference between Comparative Example 5 and Example 2 is that step (4) is different. Step (4) is changed to: hollow long and thin fibers, hollow short fibers, hollow thick long fibers, and hollow short fibers are mixed to obtain a water-soluble temporary plugging agent for acid fracturing of oil and water wells; the mass ratio of the hollow long and thin fibers, hollow short fibers, hollow thick long fibers, and hollow short fibers is 1:1:1:1; the remaining steps are the same as in Example 2.
[0051] Effect example
[0052] Table 1 below shows the performance analysis results of the water-soluble temporary plugging agents used for acid fracturing of oil and water wells using Examples 1 to 3 of the present invention and Comparative Examples 1 to 5.
[0053] Table 1
[0054]
[0055] From the comparison of the experimental results of the embodiment and the comparative example in Table 1, it can be found that the present invention utilizes the irradiation of starch and carboxymethyl cellulose, and with the assistance of sodium trimetaphosphate, promotes cross-linking between the two, and stimulates the active reaction points on the surface of cellulose through microwave effect, so that the carboxymethyl group penetrates from the surface of starch particles from the outside to the inside, and at the same time introduces a covalent bond with a stronger force than the hydrogen bond, and connects the molecules in the form of a bridge to form a network structure, thereby improving the thermal stability of starch and the water absorption rate of the matrix. Then, a scaffolding effect is provided in the amino acid-acrylamide interpenetrating structure to form a copolymer with a certain spatial network structure, so that it has an appropriate solubility at high temperature, and air is used as The core layer is made of hollow fine fibers and hollow coarse fibers through coaxial spinning, making it easier to fit and fill uneven cracks or wormholes, thereby increasing its own specific surface area and enhancing its water absorption capacity, thereby preventing the acidizing fluid from entering the high permeability area and improving the effective utilization rate of the acidizing fluid. At the same time, through shearing, hollow fine fibers and hollow coarse fibers of different lengths are made to avoid mutual entanglement due to aggregation, and the copolymer is made into granules, which has a certain compaction effect on the fibers. Under the action of pressure difference, the coarse and short fibers first form bridges at the pore throats, and gradually form temporary plugging zones with extremely poor permeability, thereby causing changes in the stress field around the temporary plugging layer, and achieving the purpose of assisting repeated fracturing crack diversion.
[0056] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A water-soluble temporary plugging agent for acid fracturing of oil and water wells, characterized in that: The water-soluble temporary plugging agent for oil and water well acid fracturing is prepared by mixing starch cross-linked carboxymethyl cellulose with an amino acid-acrylamide polymer, and then mixing the granules with fibers through a process; The fibers are specifically hollow long and thin fibers, hollow short and thin fibers, hollow thick and long fibers, and hollow thick and short fibers; The method for preparing the water-soluble temporary plugging agent for acid fracturing of oil and water wells comprises the following preparation steps: (1) Carboxymethyl cellulose and deionized water are mixed, stirred at 25-35°C and 80-130 rpm for 20-60 min, potato starch aqueous solution, sodium trimetaphosphate and anhydrous sodium sulfate are added, nitrogen is introduced at 10 mL / min, microwave cross-linking is performed at a power of 280-420 W for 5-15 min, then the mixture is immersed in methanol for 4 h, dried at 50-80°C for 10-16 h, and crushed through an 80-mesh sieve to obtain starch-cross-linked carboxymethyl cellulose; the potato starch aqueous solution contains 40% by weight of potato starch; (2) Mix polyacrylamide, amino acid and deionized water, heat to 60°C, stir at 60-100 rpm for 50-80 min, add potassium persulfate, sodium diisobutylnaphthalene sulfonate, urea and starch cross-linked carboxymethyl cellulose, heat to 60-90°C, react for 4-10 h to obtain a copolymer; (3) The copolymer was heated to 70-100°C and air was used as the core for coaxial spinning. The parameters were as follows: the inner needle diameter was 0.56 mm, the outer needle diameters were 2.01 mm and 4.21 mm, respectively, the receiving distance was 20 cm, and the feed rate was 20-50 mL / h, to obtain hollow coarse fibers and hollow fine fibers. Subsequently, hollow fine long fibers, hollow fine short fibers, hollow coarse long fibers, and hollow coarse short fibers were obtained by shearing, respectively. (4) The copolymer is ground and passed through a 20-200 mesh sieve to obtain particles, which are then mixed with hollow long and thin fibers, hollow short and thin fibers, hollow thick and long fibers, and hollow thick and short fibers to obtain a water-soluble temporary plugging agent for acid fracturing of oil and water wells.
2. The water-soluble temporary plugging agent for acid fracturing of oil and water wells according to claim 1, characterized in that: The mass ratio of the carboxymethyl cellulose, deionized water, potato starch aqueous solution, sodium trimetaphosphate and anhydrous sodium sulfate in step (1) is 0.1-0.8:3-5:2:1.2-2:
1.
3. A water-soluble temporary plugging agent for acid fracturing of oil and water wells according to claim 2, characterized in that: The molecular weight of the polyacrylamide in step (2) is 2×10 6 .
4. A water-soluble temporary plugging agent for acid fracturing of oil and water wells according to claim 3, characterized in that: The mass ratio of the polyacrylamide, amino acid, deionized water, potassium persulfate, sodium diisobutylnaphthalene sulfonate, urea, and starch-cross-linked carboxymethyl cellulose in step (2) is 5:5:10~30:0.5:0.01:0.9:0.9~1.
8.
5. A water-soluble temporary plugging agent for acid fracturing of oil and water wells according to claim 4, characterized in that: In step (3), the length of the long fiber is 10 mm, and the length of the short fiber is 1 mm.
6. A water-soluble temporary plugging agent for acid fracturing of oil and water wells according to claim 5, characterized in that: In step (4), the mass ratio of the particles, hollow long fibers, hollow short fibers, hollow thick long fibers, and hollow thick short fibers is 0.9-3:1:1:1:1.