Preparation method of high-performance composite modified polypropylene particles
The flame retardant filler is prepared by lignin and layered double hydroxide, and the intercalation layer is used to modify the concave and convex rod soil to form an inorganic-organic hybrid composite material, which solves the problem of poor compatibility of inorganic filler in polypropylene material, and realizes the High thermal stability and flame retardancy improve the overall performance of polypropylene particles.
Patent Information
- Application Number
- CN202411355218.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-09-27
AI Technical Summary
The poor compatibility between inorganic fillers and polypropylene in existing flame retardant polypropylene materials leads to uneven dispersion and poor stability, insufficient flame retardant performance, and difficult to meet high performance needs.
Flame retardant fillers are prepared by lignin and layered double hydroxide, and the concave and convex rod soil is modified by intercalation to form an inorganic-organic hybrid composite material, which improves the flame retardant and high-temperature resistance of polypropylene particles.
The high thermal stability and flame retardant effect of polypropylene particles are achieved, the overall performance is improved, and the preparation needs of high-performance composite modified polypropylene are met.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polypropylene, in particular to a method for preparing high-performance composite modified polypropylene particles. Background Art
[0002] Polypropylene is a polymer formed by the addition polymerization of propylene. It is a white waxy material with a transparent and light appearance. It is a safe and non-toxic thermoplastic synthetic resin with excellent mechanical properties. It has chemical resistance, heat resistance, electrical insulation, high-strength mechanical properties and good high-wear processing properties. It has been widely used in many fields such as clothing, fiber products, medical equipment, automobiles, bicycles, parts, pipelines, food, chemical containers, etc.
[0003] However, the flammable characteristics of this type of resin material lead to certain safety hazards, which also limits its application space and hinders the further development of polypropylene resin. In the existing flame-retardant polypropylene materials, the means of adding flame retardants and other ingredients are usually adopted to improve the flame retardant performance. However, the compatibility between inorganic fillers and polypropylene is poor, resulting in uneven distribution and poor stability. Increasing the amount of fillers added will cause the comprehensive performance of polypropylene materials to decrease. Therefore, there are still many defects, which is difficult to meet the needs of consumers. The present invention improves the dispersibility and compatibility of attapulgite in polypropylene through intercalation modification to improve the comprehensive performance of polypropylene particles, and at the same time combines composite flame retardant materials to provide a method for preparing high-performance composite modified polypropylene particles to solve the above problems. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing high-performance composite modified polypropylene particles to solve the problems existing in the prior art.
[0005] In order to solve the above technical problems, the present invention provides the following technical solution: a method for preparing high-performance composite modified polypropylene particles, comprising the following preparation steps:
[0006] (1) Lignin and deionized water are proportioned to form a lignin solution with a concentration of 30 wt%, and then air is compressed into an air distributor in a reactor through an air compressor, and the air is fully mixed with the lignin solution under stirring at a stirring speed of 350-550 rpm, a composite catalyst is added to the lignin solution, and the reaction is carried out at 50-140° C. for 30-480 min to obtain a carboxylated lignin solution; 0.5-1.5 parts of aluminum nitrate are slowly added to 5-10 parts of the carboxylated lignin solution, and after mixing, the aluminum nitrate is fully stirred at 100 rpm for 20-40 min to dissolve the aluminum nitrate, and the dissolved mixed solution is vigorously stirred at 80-100° C. for 18-30 h. After the reaction is completed, the precipitate is filtered and washed with deionized water for 3 times, and then dried at room temperature and pressure for 24 h to obtain a flame retardant filler;
[0007] (2) Under the protection of inert gas, evacuate to -0.085MPa, and then heat the attapulgite to 70-400°C for dehydroxylation treatment for 2-12h to obtain pretreated attapulgite; mix the pretreated attapulgite with citric acid in proportion, first ultrasonicate at 20kHz for 30min, and then stir at 70-90°C at 200rpm for 12h to obtain open-layer attapulgite; dissolve 0.008-0.014 parts of the catalyst in 50 parts of toluene, and stir at 100rpm for 20min to obtain a catalytic solution; place 0.5 parts of the open-layer attapulgite in a round-bottom three-necked flask connected to a condenser, evacuate to 1.5kPa to replace the inert gas protection, add 50 parts of toluene, and stir at 100rpm for 20min to obtain an attapulgite suspension; drop the obtained catalytic solution into the attapulgite suspension, and the volume ratio of the two solutions is 1: 1. The dripping is controlled within 30 minutes. After the dripping is completed, the mixture is heated to reflux for reaction for 6-10 hours at a temperature of 40°C. After the reaction is completed, the mixture is filtered, and then washed with toluene at 40°C for 10 minutes by stirring. After repeating 3 times, the mixture is evacuated to 0.085MPa and dried at room temperature for 4 hours to obtain modified attapulgite. Propylene is introduced into a three-necked flask replaced with nitrogen and propylene, and then 100 parts of toluene are added. The propylene pressure in the flask is maintained at 770mmHg and the temperature is 50-90°C under stirring at a speed of 60rpm. 0.001-0.005 parts of a catalyst are added. After stirring at the original speed for 2-10 minutes, 0.2-0.4 parts of modified attapulgite are added. After reacting for 40-120 minutes, acidified ethanol is added to terminate the polymerization reaction, and the mixture is washed with toluene in the same manner as above, and then dried at room temperature under vacuum at 0.085MPa for 6-8 hours to obtain a polypropylene-attapulgite composite.
[0008] (3) Putting an antioxidant, polypropylene wax, polypropylene-attapulgite composite and flame retardant filler into a rotary mixer in a mass ratio of 0.2-0.6:20:5-10:2-5 and mixing for 10-20 minutes, the speed of the melt rotary mixer is 70-110 rpm, and the mixture is melt-granulated at a temperature of 180-210° C. using a twin-screw extruder to obtain modified polypropylene particles.
[0009] Furthermore, it is characterized in that the pressure during the carboxylation reaction in step (1) is maintained at 0.02-1.0 MPa.
[0010] Furthermore, it is characterized in that in step (1), the mass ratio of the composite catalyst to the lignin solution is 1-3:40.
[0011] Furthermore, it is characterized in that the preparation method of the composite catalyst in step (1) is: cerium acetate, cobalt octoate and deionized water are mixed in a mass ratio of 1:3-10:200, and stirred at a speed of 60 rpm for 10 minutes to obtain the composite catalyst.
[0012] Furthermore, the stirring speed of the vigorous stirring in step (1) is 800-1200 rpm.
[0013] Furthermore, in the step (2), the inert gas is nitrogen.
[0014] Furthermore, in the step (2), the mass ratio of attapulgite to citric acid is 10:0.5-2.5.
[0015] Furthermore, the catalyst in step (2) is a Ziegler catalyst.
[0016] Furthermore, in the step (2), the solid-to-liquid ratio during toluene washing is 1:5.
[0017] Furthermore, the antioxidant in step (3) is a compound of antioxidant 1010 and antioxidant 168 in a mass ratio of 5:4.
[0018] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0019] The invention uses lignin and layered double hydroxide to prepare flame retardant filler, and uses propylene intercalated attapulgite as raw materials to mix and prepare polypropylene particles, so as to achieve high temperature resistance and flame retardant effects.
[0020] Firstly, a large number of phenolic hydroxyl groups and aldehyde groups contained in the molecular structure of lignin are utilized, air is used as an oxidant, and lignin is oxidized in the presence of cobalt salt as a catalyst, so that part of the alcoholic hydroxyl groups and aldehyde groups are oxidized into carboxyl groups, and the retained phenolic hydroxyl groups achieve the effect of high temperature resistance due to the strong capture of free radicals; aluminum nitrate is added to the carboxylated lignin and cobalt salt, and the nitrate groups react and combine with the carboxyl groups, and react with the cobalt salt at the same time to form a metal layered double hydroxide precipitate that combines with the surface of lignin to form a flame retardant filler; lignin is rich in carbon content and can be used as a carbon source during thermal decomposition. It has a strong carbon-forming ability during combustion and can prevent the combustion of olefin polymers. Combined with the metal hydroxide on the surface of lignin, the metal ions can react with the free radicals in the gas during the combustion process to form relatively stable compounds, and synergistically achieve double-effect flame retardancy;
[0021] Secondly, attapulgite has a special fibrous porous crystal structure, and making full use of its structure in polypropylene particles can achieve high thermal stability and flame retardant effects; however, the dispersibility and bonding degree of attapulgite in polypropylene are not high, so the present invention uses a catalyst citric acid to enter the interlayer of attapulgite clay, so that the interlayer spacing of the attapulgite clay increases or the layers are peeled off, and then propylene monomer is intercalated into the expanded attapulgite, and then polymerized to form an inorganic-organic hybrid composite material; finally, a flame retardant filler is added to the composite material, and the attapulgite aerogel is combined with the free radicals on the surface of the flame retardant filler, so that the polypropylene particles are combined as a whole, thereby improving its flame retardancy and high temperature resistance. DETAILED DESCRIPTION
[0022] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0023] In order to more clearly illustrate the method provided by the present invention, the following examples are used to describe in detail the various index testing methods of a high-performance composite modified polypropylene particle prepared in the following examples are as follows:
[0024] High temperature resistance: The high temperature resistance of the samples prepared in the examples and comparative examples was tested according to GB / T1633-2000 “Determination of Vicat Softening Temperature (VST) of Thermoplastics”.
[0025] Flame retardancy: Performance tests were performed on the samples prepared in the examples and comparative examples, and the flame retardancy was determined according to standards such as UL-94 and GB / T5169.12-2006.
[0026] Example 1; (1) Lignin and deionized water were mixed in proportion to form a lignin solution with a concentration of 30 wt%, and then air was compressed into the air distributor in the reactor by an air compressor, the pressure was maintained at 0.02 MPa, and the lignin solution was fully mixed under stirring at a stirring speed of 350 rpm. A composite catalyst was added to the lignin solution, the mass ratio of the composite catalyst to the lignin solution was 1:40, and the reaction was carried out at 50°C for 30 min to obtain a carboxylated lignin solution; Preparation of composite catalyst The method is as follows: cerium acetate, cobalt octanoate and deionized water are mixed in a mass ratio of 1:3:200, and stirred at a speed of 60 rpm for 10 minutes to obtain a composite catalyst; 0.5 parts of aluminum nitrate are slowly added to 5 parts of carboxylated lignin solution, and after mixing, they are fully stirred at 100 rpm for 20 minutes to dissolve the aluminum nitrate, and the dissolved mixed solution is vigorously stirred at 80°C for 18 hours at a stirring speed of 800 rpm. After the reaction is completed, the precipitate is filtered and washed with deionized water for 3 times, and then dried at room temperature and pressure for 24 hours to obtain a flame retardant filler;
[0027] (2) Under the protection of nitrogen, evacuate to -0.085MPa, and then heat the attapulgite to 70°C for dehydroxylation treatment for 2 hours to obtain pretreated attapulgite; mix the pretreated attapulgite with citric acid in a mass ratio of 10:0.5, first ultrasonicate at 20kHz for 30 minutes, and then stir at 70°C at 200rpm for 12 hours to obtain open-layer attapulgite; dissolve 0.008 parts of Ziegler catalyst in 50 parts of toluene, and stir at 100rpm for 20 minutes to obtain a catalytic solution; place 0.5 parts of open-layer attapulgite in a round-bottom three-necked flask connected to a condenser, evacuate to 1.5kPa to replace nitrogen protection, add 50 parts of toluene, and stir at 100rpm for 20 minutes to obtain an attapulgite suspension; add the obtained catalytic solution dropwise to the attapulgite suspension, and the volume ratio of the two solutions is 1:1, the addition was controlled within 30 minutes. After the addition was completed, the mixture was heated to reflux for reaction for 6 hours at a temperature of 40°C. After the reaction was completed, the mixture was filtered and then washed with toluene at 40°C for 10 minutes with a solid-liquid ratio of 1:5. After repeating 3 times, the mixture was evacuated to 0.085MPa and dried at room temperature for 4 hours to obtain modified attapulgite. Propylene was introduced into a three-necked flask replaced with nitrogen and propylene, and then 100 parts of toluene were added. The propylene pressure in the bottle was kept at 770mmHg and the temperature was 50°C under stirring at a speed of 60rpm. 0.001 parts of Ziegler catalyst were added. After stirring at the original speed for 2 minutes, 0.2 parts of modified attapulgite were added. After reacting for 40 minutes, acidified ethanol was added to terminate the polymerization reaction, and the mixture was washed with toluene in the same manner as above, and then dried at room temperature under vacuum at 0.085MPa for 6 hours to obtain a polypropylene-attapulgite composite.
[0028] (3) Antioxidant 1010 and antioxidant 168 are compounded in a mass ratio of 5:4 to form an antioxidant; antioxidant, polypropylene wax, polypropylene-attapulgite composite and flame retardant filler are placed in a rotary mixer in a mass ratio of 0.2:20:5:2 and mixed for 10 minutes. The speed of the melt rotary mixer is 70 rpm. The mixture is melt-granulated at 180°C using a twin-screw extruder to obtain modified polypropylene particles.
[0029] Example 2: (1) Lignin and deionized water are mixed in proportion to form a lignin solution with a concentration of 30 wt%, and then air is compressed into an air distributor in a reactor through an air compressor, the pressure is maintained at 0.5 MPa, and the air is fully mixed with the lignin solution under stirring at a stirring speed of 450 rpm. A composite catalyst is added to the lignin solution, the mass ratio of the composite catalyst to the lignin solution is 2:40, and the reaction is carried out at 95°C for 250 min to obtain a carboxylated lignin solution; Preparation method of composite catalyst The method comprises the following steps: mixing cerium acetate, cobalt octanoate and deionized water in a mass ratio of 1:6.5:200, and stirring at a speed of 60 rpm for 10 minutes to obtain a composite catalyst; slowly adding 1 part of aluminum nitrate to 7.5 parts of a carboxylated lignin solution, stirring at 100 rpm for 30 minutes after mixing to dissolve the aluminum nitrate, and vigorously stirring the mixed solution at 90° C. for 24 hours at a stirring speed of 1000 rpm. After the reaction is completed, filtering and collecting the precipitate, washing it with deionized water for 3 times, and drying it at room temperature and pressure for 24 hours to obtain a flame retardant filler;
[0030] (2) Under the protection of nitrogen, evacuate to -0.085MPa, and then heat the attapulgite to 235℃ for dehydroxylation treatment for 7h to obtain pretreated attapulgite; mix the pretreated attapulgite with citric acid in a mass ratio of 10:1.5, first ultrasonicate at 20kHz for 30min, and then stir at 80℃ at 200rpm for 12h to obtain open-layer attapulgite; dissolve 0.011 parts of Ziegler catalyst in 50 parts of toluene, and stir at 100rpm for 20min to obtain a catalytic solution; place 0.5 parts of open-layer attapulgite in a round-bottom three-necked flask connected to a condenser, evacuate to 1.5kPa to replace nitrogen protection, add 50 parts of toluene, and stir at 100rpm for 20min to obtain an attapulgite suspension; add the obtained catalytic solution dropwise to the attapulgite suspension, and the volume ratio of the two solutions is 1:1, the addition was controlled within 30 minutes. After the addition was completed, the reaction was heated to reflux for 8 hours at a temperature of 40°C. After the reaction was completed, it was filtered, and then washed with toluene at 40°C for 10 minutes with a solid-liquid ratio of 1:5. After repeating 3 times, it was evacuated to 0.085MPa and dried at room temperature for 4 hours to obtain modified attapulgite; propylene was introduced into a three-necked flask replaced with nitrogen and propylene, and then 100 parts of toluene were added. The propylene pressure in the bottle was kept at 770mmHg and the temperature was 70°C under stirring at 60rpm. 0.003 parts of Ziegler catalyst were added, and the original stirring speed was maintained for 6 minutes. 0.3 parts of modified attapulgite were added. After reacting for 80 minutes, acidified ethanol was added to terminate the polymerization reaction, and it was washed with toluene in the same way as above, and then dried at room temperature under vacuum at 0.085MPa for 7 hours to obtain a polypropylene-attapulgite composite;
[0031] (3) Antioxidant 1010 and antioxidant 168 are compounded in a mass ratio of 5:4 to form an antioxidant; antioxidant, polypropylene wax, polypropylene-attapulgite composite and flame retardant filler are placed in a rotary mixer in a mass ratio of 0.4:20:7.5:3.5 and mixed for 15 minutes. The speed of the melt rotary mixer is 90 rpm. The mixture is melt-granulated at a temperature of 195°C using a twin-screw extruder to obtain modified polypropylene particles.
[0032] Example 3; (1) Lignin and deionized water are mixed in proportion to form a lignin solution with a concentration of 30wt%, and then air is compressed into an air distributor in a reactor through an air compressor, the pressure is maintained at 1.0MPa, and the air is fully mixed with the lignin solution under stirring at a stirring speed of 550rpm, and a composite catalyst is added to the lignin solution, the mass ratio of the composite catalyst to the lignin solution is 3:40, and the reaction is carried out at 140°C for 480min to obtain a carboxylated lignin solution; Preparation method of composite catalyst The method comprises the following steps: mixing cerium acetate, cobalt octanoate and deionized water in a mass ratio of 1:10:200, and stirring at a speed of 60 rpm for 10 minutes to obtain a composite catalyst; slowly adding 1.5 parts of aluminum nitrate to 10 parts of a carboxylated lignin solution, and stirring the mixture at 100 rpm for 40 minutes to dissolve the aluminum nitrate. The dissolved mixed solution is vigorously stirred at 100° C. for 30 hours at a stirring speed of 1200 rpm. After the reaction is completed, the precipitate is filtered out, washed with deionized water for 3 times, and dried at room temperature and pressure for 24 hours to obtain a flame retardant filler.
[0033] (2) Under the protection of nitrogen, evacuate to -0.085MPa, and then heat the attapulgite to 400℃ for dehydroxylation for 12h to obtain pretreated attapulgite; mix the pretreated attapulgite with citric acid in a mass ratio of 10:2.5, first ultrasonicate at 20kHz for 30min, and then stir at 90℃ at 200rpm for 12h to obtain open-layer attapulgite; dissolve 0.014 parts of Ziegler catalyst in 50 parts of toluene, and stir at 100rpm for 20min to obtain a catalytic solution; place 0.5 parts of open-layer attapulgite in a round-bottom three-necked flask connected to a condenser, evacuate to 1.5kPa to replace nitrogen protection, add 50 parts of toluene, and stir at 100rpm for 20min to obtain an attapulgite suspension; add the obtained catalytic solution dropwise to the attapulgite suspension, and the volume ratio of the two solutions is 1:1. :1, the addition was controlled within 30 minutes. After the addition was completed, the mixture was heated to reflux for reaction for 10 hours at a temperature of 40°C. After the reaction was completed, the mixture was filtered and then washed with toluene at 40°C for 10 minutes with a solid-liquid ratio of 1:5. After repeated 3 times, the mixture was evacuated to 0.085MPa and dried at room temperature for 4 hours to obtain modified attapulgite. Propylene was introduced into a three-necked flask replaced with nitrogen and propylene, and then 100 parts of toluene were added. The propylene pressure in the bottle was maintained at 770mmHg and the temperature was 90°C under stirring at a speed of 60rpm. 0.005 parts of Ziegler catalyst were added. After stirring at the original speed for 10 minutes, 0.4 parts of modified attapulgite were added. After the reaction was completed for 120 minutes, acidified ethanol was added to terminate the polymerization reaction, and the mixture was washed with toluene in the same manner as above, and then dried at room temperature under vacuum at 0.085MPa for 8 hours to obtain a polypropylene-attapulgite composite.
[0034] (3) Antioxidant 1010 and antioxidant 168 are compounded in a mass ratio of 5:4 to form an antioxidant; antioxidant, polypropylene wax, polypropylene-attapulgite composite and flame retardant filler are placed in a rotary mixer in a mass ratio of 0.6:20:10:5 and mixed for 20 minutes. The speed of the melt rotary mixer is 110 rpm. The mixture is melt-granulated at 210° C. using a twin-screw extruder to obtain modified polypropylene particles.
[0035] Comparative Example 1: The difference between Comparative Example 1 and Example 2 is that step (1) is different, and step (1) is changed to: lignin and deionized water are configured in proportion to form a lignin solution with a concentration of 30wt%; the preparation method of the composite catalyst is: cerium acetate, cobalt octoate and deionized water are mixed in a mass ratio of 1:6.5:200, and stirred at 60rpm for 10min to obtain a composite catalyst; 1 part of aluminum nitrate is slowly added to 7.5 parts of the lignin solution, and after mixing, it is fully stirred at 100rpm for 30min to dissolve the aluminum nitrate. The dissolved mixed solution is vigorously stirred at 90°C for 24h, and the stirring speed is 1000rpm. After the reaction is completed, the precipitate is filtered and washed with deionized water 3 times, and then dried at room temperature and pressure for 24h to obtain a flame retardant filler; the remaining steps are the same as Example 2.
[0036] Comparative Example 2: The difference between Comparative Example 2 and Example 2 is that step (1) is omitted, and step (3) is changed to: antioxidant 1010 and antioxidant 168 are compounded into an antioxidant in a mass ratio of 5:4; antioxidant, polypropylene wax, polypropylene-attapulgite composite, lignin, and talc are placed in a rotary mixer in a mass ratio of 0.4:20:7.5:2:1.5 and mixed for 15 minutes, the speed of the melt rotary mixer is 90 rpm, and the mixture is melt-granulated at a temperature of 195°C using a twin-screw extruder to obtain modified polypropylene particles; the remaining steps are the same as in Example 2.
[0037] Comparative Example 3 (without addition of hydroxide) The difference between Comparative Example 3 and Example 2 is that step (1) is different. Step (1) is changed to: lignin and deionized water are proportionally configured to form a lignin solution with a concentration of 30wt%, and then air is compressed into the air distributor in the reactor through an air compressor, the pressure is maintained at 0.5MPa, and the lignin solution is fully mixed under stirring at a stirring speed of 450rpm. A composite catalyst is added to the lignin solution, the mass ratio of the composite catalyst to the lignin solution is 2:40, and the reaction is carried out at 95°C for 250min. After the reaction is completed, the precipitate is filtered and washed with deionized water 3 times, and then dried at room temperature and pressure for 24h to obtain a flame retardant filler; the remaining steps are the same as Example 2.
[0038] Comparative Example 4; The difference between Comparative Example 4 and Example 2 is that there is no step (2), and step (3) is changed to: antioxidant 1010 and antioxidant 168 are compounded into an antioxidant in a mass ratio of 5:4; the antioxidant, polypropylene wax, attapulgite composite and flame retardant filler are put into a rotary mixer in a mass ratio of 0.4:25:4.5:3.5 and mixed for 15 minutes, the speed of the melt rotary mixer is 90 rpm, and the mixture is melt-granulated at a temperature of 195°C using a twin-screw extruder to obtain modified polypropylene particles; the remaining steps are the same as Example 2.
[0039] Comparative Example 5; The difference between Comparative Example 5 and Example 2 is that step (2) is different, and step (2) is changed to: dissolve 0.011 parts of Ziegler catalyst in 50 parts of toluene, stir at 100 rpm for 20 minutes to obtain a catalytic solution; place 0.5 parts of attapulgite in a round-bottom three-necked flask connected to a condenser, evacuate to 1.5 kPa to replace nitrogen protection, add 50 parts of toluene, and stir at 100 rpm for 20 minutes to obtain a attapulgite suspension; add the prepared catalytic solution dropwise to the attapulgite suspension, the volume ratio of the two solutions is 1:1, and the addition is controlled within 30 minutes. After the addition is completed, heat and reflux for 8 hours at a temperature of 40°C. After the reaction is completed, filter and stir with toluene at 40°C. Wash for 10 minutes with a solid-liquid ratio of 1:5, repeat 3 times, evacuate to 0.085 MPa and dry at room temperature for 4 hours to obtain modified attapulgite; introduce propylene into a three-necked flask replaced with nitrogen and propylene, then add 100 parts of toluene, keep the propylene pressure in the bottle at 770 mmHg and the temperature at 70°C under stirring at 60 rpm, add 0.003 parts of Ziegler catalyst, keep stirring at the original speed for 6 minutes, add 0.3 parts of modified attapulgite, react for 80 minutes, add acidified ethanol to terminate the polymerization reaction, wash with toluene in the same way as above, and then dry at room temperature under vacuum at 0.085 MPa for 7 hours to obtain a polypropylene-attapulgite composite; the remaining steps are the same as Example 2.
[0040] Effect example
[0041] Table 1 below shows the performance analysis results of a high-performance composite modified polypropylene particle using Examples 1 to 3 of the present invention and Comparative Examples 1 to 5.
[0042] Table 1
[0043] Flame retardant / 1.6mm Microcaloric softening temperature / ℃ Example 1 V0 162 Example 2 V0 165 Example 3 V0 164 Comparative Example 1 V1 135 Comparative Example 2 V1 138 Comparative Example 3 V2 125 Comparative Example 4 V1 145 Comparative Example 5 V1 140
[0044] From the comparison of the experimental data of high temperature resistance of the embodiment and the comparative example, it can be found that the present invention utilizes a large number of phenolic hydroxyl groups and aldehyde groups contained in the molecular structure of lignin, uses air as an oxidant, and oxidizes lignin in the presence of cobalt salt as a catalyst, oxidizing part of the alcoholic hydroxyl groups and aldehyde groups into carboxyl groups, and the retained phenolic hydroxyl groups achieve the effect of high temperature resistance due to the strong capture of free radicals. From the comparison of the experimental data of flame retardancy of the embodiment and the comparative example, it can be found that the present invention adds aluminum nitrate to the carboxylated lignin and cobalt salt, and the nitrate group reacts with the carboxyl group and reacts with the cobalt salt to form a metal layered double hydroxide precipitate that is combined with the surface of lignin to form a flame retardant filler; lignin is rich in carbon content and can be used as a carbon source during thermal decomposition. It has a strong carbon-forming ability during combustion and can prevent the combustion of olefin polymers. Combined with the metal hydroxide on the surface of lignin, the metal ions can react with the free radicals in the gas during the combustion process to form relatively stable compounds, synergistic double-effect flame retardant; the added attapulgite has special The special fibrous porous crystal structure of attapulgite can be fully utilized to achieve high thermal stability and flame retardant effect in polypropylene particles, but the dispersibility and bonding degree of attapulgite in polypropylene are not high, so the present invention uses catalyst citric acid to enter the interlayer of attapulgite clay, so that the interlayer distance of attapulgite clay is increased or the layers are peeled off, and then propylene monomer is intercalated into the expanded attapulgite, and then polymerized to form an inorganic-organic hybrid composite material; finally, the flame retardant filler is added to the composite material, and the attapulgite aerogel is combined with the free radicals on the surface of the flame retardant filler, so that the polypropylene particles are combined as a whole, thereby improving its flame retardancy and high temperature resistance.
[0045] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A method for preparing high-performance composite modified polypropylene particles, It is characterized in that The method comprises the following preparation steps: (1) Lignin and deionized water are proportioned to form a lignin solution with a concentration of 30 wt%, and then air is compressed into an air distributor in a reactor through an air compressor, and the air is fully mixed with the lignin solution under stirring at a stirring speed of 350-550 rpm, a composite catalyst is added to the lignin solution, and the reaction is carried out at 50-140° C. for 30-480 min to obtain a carboxylated lignin solution; 0.5-1.5 parts of aluminum nitrate are slowly added to 5-10 parts of the carboxylated lignin solution, and after mixing, the aluminum nitrate is fully stirred at 100 rpm for 20-40 min to dissolve the aluminum nitrate, and the dissolved mixed solution is vigorously stirred at 80-100° C. for 18-30 h. After the reaction is completed, the precipitate is filtered and washed with deionized water for 3 times, and then dried at room temperature and pressure for 24 h to obtain a flame retardant filler; (2) Under the protection of inert gas, evacuate to -0.085MPa, and then heat the attapulgite to 70-400°C for dehydroxylation treatment for 2-12h to obtain pretreated attapulgite; mix the pretreated attapulgite with citric acid in proportion, first ultrasonicate at 20kHz for 30min, and then stir at 70-90°C at 200rpm for 12h to obtain open-layer attapulgite; dissolve 0.008-0.014 parts of the catalyst in 50 parts of toluene, and stir at 100rpm for 20min to obtain a catalytic solution; place 0.5 parts of the open-layer attapulgite in a round-bottom three-necked flask connected to a condenser, evacuate to 1.5kPa to replace the inert gas protection, add 50 parts of toluene, and stir at 100rpm for 20min to obtain an attapulgite suspension; drop the obtained catalytic solution into the attapulgite suspension, and the volume ratio of the two solutions is 1:
1. The dripping is controlled within 30 minutes. After the dripping is completed, the mixture is heated to reflux for reaction for 6-10 hours at a temperature of 40°C. After the reaction is completed, the mixture is filtered, and then washed with toluene at 40°C for 10 minutes by stirring. After repeating 3 times, the mixture is evacuated to 0.085MPa and dried at room temperature for 4 hours to obtain modified attapulgite. Propylene is introduced into a three-necked flask replaced with nitrogen and propylene, and then 100 parts of toluene are added. The propylene pressure in the flask is maintained at 770mmHg and the temperature is 50-90°C under stirring at a speed of 60rpm. 0.001-0.005 parts of a catalyst are added. After stirring at the original speed for 2-10 minutes, 0.2-0.4 parts of modified attapulgite are added. After reacting for 40-120 minutes, acidified ethanol is added to terminate the polymerization reaction, and the mixture is washed with toluene in the same manner as above, and then dried at room temperature under vacuum at 0.085MPa for 6-8 hours to obtain a polypropylene-attapulgite composite. (3) Putting an antioxidant, polypropylene wax, polypropylene-attapulgite composite and flame retardant filler into a rotary mixer in a mass ratio of 0.2-0.6:20:5-10:2-5 and mixing for 10-20 minutes, the speed of the melt rotary mixer is 70-110 rpm, and the mixture is melt-granulated at a temperature of 180-210° C. using a twin-screw extruder to obtain modified polypropylene particles.
2. A method for preparing high-performance composite modified polypropylene particles according to claim 1, It is characterized in that The pressure during the carboxylation reaction in step (1) is maintained at 0.02-1.0 MPa.
3. The method for preparing high-performance composite modified polypropylene particles according to claim 1, It is characterized in that In the step (1), the mass ratio of the composite catalyst to the lignin solution is 1-3:
40.
4. The method for preparing high-performance composite modified polypropylene particles according to claim 1, It is characterized in that The preparation method of the composite catalyst in step (1) is as follows: cerium acetate, cobalt octoate and deionized water are mixed in a mass ratio of 1:3-10:200, and stirred at a speed of 60 rpm for 10 minutes to obtain the composite catalyst.
5. The method for preparing high-performance composite modified polypropylene particles according to claim 1, It is characterized in that The stirring speed of the vigorous stirring in step (1) is 800-1200 rpm.
6. The method for preparing high-performance composite modified polypropylene particles according to claim 1, It is characterized in that The inert gas in step (2) is nitrogen.
7. The method for preparing high-performance composite modified polypropylene particles according to claim 1, It is characterized in that In the step (2), the mass ratio of attapulgite to citric acid is 10:0.5-2.
5.
8. The method for preparing high-performance composite modified polypropylene particles according to claim 1, It is characterized in that The catalyst in step (2) is a Ziegler catalyst.
9. The method for preparing high-performance composite modified polypropylene particles according to claim 1, It is characterized in that In the step (2), the solid-to-liquid ratio during toluene washing is 1:
5.
10. The method for preparing high-performance composite modified polypropylene particles according to claim 1, It is characterized in that The antioxidant in step (3) is a compound of antioxidant 1010 and antioxidant 168 in a mass ratio of 5:4.
Citation Information
Patent Citations
Modified polyolefins
CN102695726A
Nano-polypropylene flame retardant plastic
CN103467854A
Preparation method of expanded flame-retardant polypropylene composite material
CN108676254A
Conductive foam material with good flame retardance and preparation method thereof
CN115028984A
Modified-layered-silicate-basedaldehyde-free flame-retardant adhesive and application thereof