Preparation process of high-hardness polyurea coating anti-explosion coating material

By adding glass fibers and flame retardants to the polyurea coating, the problem of poor flame retardant performance of the existing polyurea coating is solved, the explosion resistance and flame retardant performance of the coating is improved, and high hardness and efficient fire resistance are achieved. Effect.

CN118995016AInactive Publication Date: 2024-11-22SHANDONG DES-LEAD ADVANCED MATERIALS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411244749.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing polyurea coating has poor flame retardant properties and is difficult to meet the requirements of high hardness and explosion resistance.

Method used

The mechanical strength and flame retardant properties of the coating are improved by adding glass fibers and flame retardant to the polyurea coating. The specific steps include preheating the isocyanate prepolymer, end amino polyether and chain extender, mixing it uniformly with the flame retardant and antifouling agent at a specific temperature and pressure to form a high-hardness polyurea coating anti-explosion coating. Material.

Benefits of technology

Improve the explosion resistance and flame retardant properties of the coating, enhance the mechanical strength through the addition of glass fibers, and suppress the flame and reduce the generation of combustible gases by adding flame retardant, forming oxide particles with porous structures to prevent heat transfer .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118995016A_ABST
    Figure CN118995016A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation process of a high-hardness polyurea coating anti-explosion coating material, and relates to the technical field of polyurea coating compositions. According to the preparation process of the high-hardness anti-explosion coating material of the polyurea coating, the flame retardant is added, PO. Free radicals released by polyphosphazene can be combined with hydrogen atoms in a flame area in the combustion process, the flame inhibition effect is achieved, phosphoric acid, metaphosphoric acid and polymetaphosphoric acid generated by combustion of polyphosphazene can promote dehydration and carbonization of polyurea, and the anti-explosion coating material of the high-hardness anti-explosion coating material of the polyurea coating can be used for preparing the anti-explosion coating material of the high-hardness anti-explosion coating material of the polyurea coating. The amount of combustible gas generated in the polyurea thermal decomposition process is reduced, the flame retardant effect is achieved, meanwhile, in the combustion process, degradation of the flame retardant can generate oxide particles of a porous structure, heat transmission can be prevented, charring can be promoted, and the formed carbon structure is compact and not prone to combustion, so that the flame retardant has a good flame retardant effect. The flame retardant property of the polyurea coating is effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyurea coating compositions, in particular to a preparation process of a high-hardness polyurea coating anti-explosion coating material. Background Art

[0002] Polyurea is an elastomeric substance generated by the reaction of isocyanate and amino compounds. Compared with traditional coatings, it has the following advantages: good inertness, not affected by ambient temperature and humidity during construction; no volatile organic compounds, environmentally friendly; good material adhesion, can be sprayed on concrete, metal plates, wood and other substrates; no catalyst, can achieve rapid curing, spray without sagging, can be sprayed on various shapes of surfaces, five seconds to gel, sixty seconds to have walking strength; can be hot sprayed and poured, high construction efficiency and adjustable thickness, beautiful coating can be formed in one time.

[0003] The Chinese patent with publication number CN116285614A discloses a method for preparing a polyurea coating composition and a method for preparing an explosion-resistant and impact-resistant polyurea coating. The method for preparing the polyurea coating composition comprises the following steps: (1) after subjecting a polyether polyol to a first decompression dehydration, adding a reactive diluent to a second decompression dehydration, and after a first cooling, adding isocyanate, heating up to carry out a polymerization reaction, and subjecting the component A to a second cooling; in the component A, the -NCO content is 15.5-17wt%; (2) under stirring, a liquid amine chain extender, an amino-terminated polyether, and an optional auxiliary agent are uniformly mixed, subjected to a third decompression dehydration, filtered and packaged to obtain a component B; in terms of weight, in the component A, the amount of isocyanate is 45-52 parts, the amount of polyether polyol is 43-52 parts, and the amount of reactive diluent is 3-5 parts; in the component B: the amount of amino-terminated polyether is 57-65 parts, and the amount of liquid amine chain extender is 35-38 parts. However, the polyurea coating prepared by the above-mentioned prior art has poor flame retardant performance when in use; therefore, the present invention provides a preparation process of a high-hardness polyurea coating anti-explosion coating material to solve the above-mentioned problem. Summary of the invention

[0004] In view of the deficiencies of the prior art, the present invention provides a preparation process of a high-hardness polyurea coating explosion-proof coating material, which solves the problems mentioned in the above background technology.

[0005] To achieve the above objectives, the present invention is implemented by the following technical scheme: A preparation process of a high-hardness polyurea coating explosion-proof coating material comprises the following preparation steps:

[0006] Step 1: Preheat the isocyanate prepolymer, amino-terminated polyether, chain extender, and additive in a drying oven at 75 to 80° C. for 45 to 60 minutes to ensure that the raw materials are in a liquid state;

[0007] Step 2: After the preheating is completed, the amino-terminated polyether, the chain extender and the auxiliary agent are mixed evenly to obtain component A;

[0008] Step 3: under the temperature condition of 50-70° C. and the pressure condition of 6-10 MPa, pour the isocyanate prepolymer into the A component, and mix and coat them to obtain the high-hardness polyurea coating anti-explosion coating material;

[0009] The mass ratio of the isocyanate prepolymer to component A is (1-1.1):1;

[0010] Among them, in parts by weight, the isocyanate prepolymer is 48 to 55 parts; in the A component, the amino-terminated polyether is 55 to 65 parts, the chain extender is 32 to 35 parts, and the auxiliary agent is 2.5 to 5 parts;

[0011] The auxiliary agent comprises: 32wt%-40wt% of antifouling agent, 35wt%-46wt% of flame retardant, and 20wt%-32wt% of glass fiber.

[0012] Preferably, the amino-terminated polyether is selected from one or more of secondary amino polyether diamines and secondary amino polyether triamines.

[0013] Preferably, the -NCO content in the isocyanate prepolymer is 15.5 wt% to 17.5 wt%.

[0014] Preferably, the chain extender is selected from one or more of 3,5-diethyltoluenediamine and 4,4-bis-sec-butylaminodiphenylmethane.

[0015] Preferably, the preparation method of the antifouling agent is:

[0016] 1) Pour 30 mL of dimethyl sulfoxide into 2,4,6-triaminopyrimidine and dissolve it while stirring;

[0017] 2) At a temperature of 40-45°C, slowly add KH560 and react for 6-8 hours to obtain the antifouling agent.

[0018] Preferably, in the antifouling agent, the weight proportions of each component added are: 25 to 35 parts of 2,4,6-triaminopyrimidine and 15 to 18 parts of KH560.

[0019] Preferably, the specific preparation method of the flame retardant is:

[0020] Ⅰ. Add 0.6 to 1.5 parts of Zn(NO 3 ) 2 6H 2 0, add 80 mL of distilled water, and stir at 350-400 rpm for 20-25 min;

[0021] Ⅱ. Add 1.2-2.2 parts of NaOH, continue stirring for 15-20 minutes, place in a drying oven at 180-200°C for 18-24 hours, cool to room temperature, and then centrifuge at 6000-8000 rpm;

[0022] III. 0.08 to 0.1 parts of Co(NO 3 ) 2 6H 2 15-20 parts of solvent are poured into a mixture of 0 and 2-3 parts of 2-methylimidazole, and after dissolution, 0.4-0.6 parts of the substance obtained in step II are added, and the mixture is reacted at a temperature of 60-65°C for 1.5-2h. After the reaction is completed, the mixture is cooled to room temperature and washed with anhydrous ethanol and deionized water;

[0023] IV. Then add 90-100 mL of 1,4-dioxane, perform ultrasonic dispersion, and then add 4,4'-diaminodiphenyl ether and hexachlorocyclotriphosphazene in sequence, stir at 75-80°C for 20-24 hours, cool to room temperature, and wash with anhydrous ethanol to obtain a flame retardant.

[0024] Preferably, in III, the solvent is a mixed solution of dimethylformamide and distilled water, and the volume ratio thereof is 1:1.

[0025] Beneficial Effects

[0026] The present invention provides a preparation process of a high-hardness polyurea coating explosion-proof coating material. Compared with the prior art, it has the following beneficial effects:

[0027] (1) The preparation process of the high-hardness polyurea coating explosion-proof coating material can hinder the expansion of substrate cracks by adding glass fiber, and enhance the hydrogen bonding effect with NH groups, and increase the total hydrogen bonding degree of urea carbonyl groups. Macroscopically, it is manifested as an improvement in the mechanical strength of the coating material, thereby improving the explosion-proof performance of the coating material.

[0028] (2) The preparation process of the high-hardness polyurea coating explosion-proof coating material, through the addition of flame retardant, during the combustion process, the PO· free radicals released by polyphosphazene can combine with hydrogen atoms in the flame area to achieve the effect of suppressing the flame, and the phosphoric acid, metaphosphoric acid and polymetaphosphoric acid generated by the combustion of polyphosphazene can promote the dehydration and carbonization of polyurea, thereby reducing the amount of combustible gas generated during the thermal decomposition of polyurea, thereby achieving the flame retardant effect. At the same time, during the combustion process, the degradation of the flame retardant will produce oxide particles with a porous structure, which can prevent heat transfer and promote carbonization. The formed carbon structure is dense and not easy to burn, effectively improving the flame retardant performance of the polyurea coating. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1A comparison chart of the total heat release of the polyurea coating provided for the preparation process of the high-hardness polyurea coating anti-explosion coating material of the present invention;

[0030] Figure 2 A comparison chart of explosion tests between Comparative Example 1 and Example 1 provided for the preparation process of the high-hardness polyurea coating explosion-proof coating material of the present invention. DETAILED DESCRIPTION

[0031] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0032] Example 1

[0033] The preparation process of the high-hardness polyurea coating anti-explosion coating material includes the following preparation steps:

[0034] Step 1, 48g of isocyanate prepolymer with an -NCO content of 15.5wt%, 65g of secondary amino polyether diamine, 35g of 3,5-diethyltoluenediamine, and 5g of auxiliary agent are placed in a drying oven at 75°C and preheated for 45min to ensure that the raw materials are in liquid state;

[0035] Step 2: After the preheating is completed, the amino-terminated polyether and the additive are mixed evenly to obtain component A;

[0036] The additives include: 32wt% antifouling agent, 46wt% flame retardant, and 22wt% glass fiber;

[0037] The preparation method of the antifouling agent is as follows: pour 30 mL of dimethyl sulfoxide into 25 g of 2,4,6-triaminopyrimidine and dissolve it while stirring; slowly drop 18 g of KH560 at a temperature of 40° C. and react for 6 hours to obtain the antifouling agent;

[0038] The specific preparation method of the flame retardant is: add 0.6g of Zn(NO 3 ) 2 6H 2 0, add 80 mL of distilled water, stir at 350 rpm for 20 min; add 2.2 g of NaOH, continue stirring for 15 min, place in a drying oven at 180 ° C for 18 h, cool to room temperature, and then centrifuge at 6000 rpm to obtain substance 1; add 0.08 g of Co(NO 3 ) 2 6H 2Pour 15g of a mixed solution of dimethylformamide and distilled water in a volume ratio of 1:1 into a mixture of 0.05g and 2g of 2-methylimidazole, add 0.4g of substance 1 after dissolving, and react at a temperature of 60°C for 1.5h. After the reaction is completed, cool to room temperature and wash with anhydrous ethanol and deionized water; then add 90mL of 1,4-dioxane, perform ultrasonic dispersion, and then add 4,4'-diaminodiphenyl ether and hexachlorocyclotriphosphazene in turn, stir at a temperature of 75°C for 20h, cool to room temperature, and wash with anhydrous ethanol to obtain a flame retardant;

[0039] Step three: under the temperature condition of 50° C. and the pressure condition of 6 MPa, the isocyanate prepolymer and the component A are mixed and coated in a mass ratio of 1:1 to obtain the high-hardness polyurea coating anti-explosion coating material.

[0040] Example 2

[0041] The preparation process of the high-hardness polyurea coating anti-explosion coating material includes the following preparation steps:

[0042] Step 1, 50g of isocyanate prepolymer with an -NCO content of 16.5wt%, 60g of secondary amino polyether diamine, 33g of 3,5-diethyltoluenediamine, and 3g of auxiliary agent are placed in a drying oven at 80°C and preheated for 50min to ensure that the raw materials are in liquid state;

[0043] Step 2: After the preheating is completed, the amino-terminated polyether and the additive are mixed evenly to obtain component A;

[0044] The additives include: 35wt% antifouling agent, 40wt% flame retardant, and 25wt% glass fiber;

[0045] The preparation method of the antifouling agent is as follows: pour 30 mL of dimethyl sulfoxide into 20 g of 2,4,6-triaminopyrimidine and dissolve it while stirring; slowly drop 16 g of KH560 at a temperature of 45° C. and react for 7 hours to obtain the antifouling agent;

[0046] The specific preparation method of the flame retardant is: add 1.0g of Zn(NO 3 ) 2 6H 2 0, add 80 mL of distilled water, stir at 380 rpm for 25 min; add 1.5 g of NaOH, continue stirring for 20 min, place in a drying oven at 190 ° C for 20 h, cool to room temperature, and then centrifuge at 7000 rpm to obtain substance 1; add 0.09 g of Co(NO 3 ) 2 6H 2Pour 18g of a mixed solution of dimethylformamide and distilled water in a volume ratio of 1:1 into a mixture of 0.01g and 2.5g of 2-methylimidazole, add 0.5g of substance 1 after dissolving, and react at 65°C for 2h. After the reaction is completed, cool to room temperature and wash with anhydrous ethanol and deionized water; then add 95mL of 1,4-dioxane, perform ultrasonic dispersion, then add 4,4'-diaminodiphenyl ether and hexachlorocyclotriphosphazene in turn, stir at 80°C for 22h, cool to room temperature, and wash with anhydrous ethanol to obtain a flame retardant;

[0047] Step three: under the temperature condition of 60° C. and the pressure condition of 8 MPa, the isocyanate prepolymer and the component A are mixed and coated in a mass ratio of 1.1:1 to obtain the high-hardness polyurea coating anti-explosion coating material.

[0048] Example 3

[0049] The preparation process of the high-hardness polyurea coating anti-explosion coating material includes the following preparation steps:

[0050] Step 1, 55g of isocyanate prepolymer with an -NCO content of 17.5wt%, 55g of secondary amino polyether triamine, 32g of 4,4-bis-sec-butylaminodiphenylmethane, and 2.5g of auxiliary agent are placed in a drying oven at 80°C and preheated for 60min to ensure that the raw materials are in liquid state;

[0051] Step 2: After the preheating is completed, the amino-terminated polyether and the additive are mixed evenly to obtain component A;

[0052] The additives include: 32wt% antifouling agent, 38wt% flame retardant, and 30wt% glass fiber;

[0053] The preparation method of the antifouling agent is as follows: pour 30 mL of dimethyl sulfoxide into 35 g of 2,4,6-triaminopyrimidine and dissolve it while stirring; slowly drop 15 g of KH560 at a temperature of 45° C. and react for 8 hours to obtain the antifouling agent;

[0054] The specific preparation method of the flame retardant is: add 1.5g of Zn(NO 3 ) 2 6H 2 0, add 80 mL of distilled water, stir at 400 rpm for 25 min; add 2.2 g of NaOH, continue stirring for 20 min, place in a drying oven at 200 ° C for 24 h, cool to room temperature, and then centrifuge at 8000 rpm to obtain substance 1; add 0.1 g of Co(NO 3 ) 2 6H 2Pour 20g of a mixed solution of dimethylformamide and distilled water in a volume ratio of 1:1 into a mixture of 0.01g and 3g of 2-methylimidazole, add 0.6g of substance 1 after dissolving, and react at 65°C for 2h. After the reaction is completed, cool to room temperature and wash with anhydrous ethanol and deionized water; then add 100mL of 1,4-dioxane, perform ultrasonic dispersion, then add 4,4'-diaminodiphenyl ether and hexachlorocyclotriphosphazene in turn, stir at 75-80°C for 24h, cool to room temperature, and wash with anhydrous ethanol to obtain a flame retardant;

[0055] Step three: under the temperature condition of 70° C. and the pressure condition of 10 MPa, the isocyanate prepolymer and the component A are mixed and coated in a mass ratio of 1.1:1 to obtain the high-hardness polyurea coating anti-explosion coating material.

[0056] Comparative Example 1

[0057] The preparation process of the high-hardness polyurea coating anti-explosion coating material includes the following preparation steps:

[0058] Step 1, 48g of isocyanate prepolymer with an -NCO content of 15.5wt%, 65g of aminopolyetherdiamine, 35g of 4,4-bis-sec-butylaminodiphenylmethane, and 5g of auxiliary agent are placed in a drying oven at 75°C and preheated for 45min to ensure that the raw materials are in liquid state;

[0059] Step 2: After the preheating is completed, the amino-terminated polyether and the additive are mixed evenly to obtain component A;

[0060] The additives include: 32wt%wt% antifouling agent, 46wt% flame retardant;

[0061] The preparation method of the antifouling agent is as follows: pour 30 mL of dimethyl sulfoxide into 25 g of 2,4,6-triaminopyrimidine and dissolve it while stirring; slowly drop 18 g of KH560 at a temperature of 40° C. and react for 6 hours to obtain the antifouling agent;

[0062] The specific preparation method of the flame retardant is: add 0.6g of Zn(NO 3 ) 2 6H 2 0, add 80 mL of distilled water, stir at 350 rpm for 20 min; add 2.2 g of NaOH, continue stirring for 15 min, place in a drying oven at 180 ° C for 18 h, cool to room temperature, and then centrifuge at 6000 rpm to obtain substance 1; add 0.08 g of Co(NO 3 ) 2 6H 2Pour 15g of a mixed solution of dimethylformamide and distilled water in a volume ratio of 1:1 into a mixture of 0.05g and 2g of 2-methylimidazole, add 0.4g of substance 1 after dissolving, and react at a temperature of 60°C for 1.5h. After the reaction is completed, cool to room temperature and wash with anhydrous ethanol and deionized water; then add 90mL of 1,4-dioxane, perform ultrasonic dispersion, and then add 4,4'-diaminodiphenyl ether and hexachlorocyclotriphosphazene in turn, stir at a temperature of 75°C for 20h, cool to room temperature, and wash with anhydrous ethanol to obtain a flame retardant;

[0063] Step three: under the temperature condition of 50° C. and the pressure condition of 6 MPa, the isocyanate prepolymer and the component A are mixed and coated in a mass ratio of 1:1 to obtain the high-hardness polyurea coating anti-explosion coating material.

[0064] Comparative Example 2

[0065] The preparation process of the high-hardness polyurea coating anti-explosion coating material includes the following preparation steps:

[0066] Step 1, 48g of isocyanate prepolymer with an -NCO content of 15.5wt%, 65g of aminopolyetherdiamine, 35g of 4,4-bis-sec-butylaminodiphenylmethane, and 5g of auxiliary agent are placed in a drying oven at 75°C and preheated for 45min to ensure that the raw materials are in liquid state;

[0067] Step 2: After the preheating is completed, the amino-terminated polyether and the additive are mixed evenly to obtain component A;

[0068] The auxiliary agent includes: 50wt% copper pyrithione and 50wt% zinc borate;

[0069] Step three: under the temperature condition of 50° C. and the pressure condition of 6 MPa, the isocyanate prepolymer and the component A are mixed and coated in a mass ratio of 1:1 to obtain the high-hardness polyurea coating anti-explosion coating material.

[0070] Sample preparation: Bolt holes with a diameter of 30 mm are punched around the Q235 steel plate with a size of 75 mm × 75 mm × 10 mm, and polyurea coating is sprayed on the surface of the steel plate. The steel plate needs to be polished before spraying to enhance the adhesion between the coating and the steel plate. A layer of primer is applied to the surface of the polished steel plate. The purpose of applying the primer is also to improve the adhesion between the steel plate substrate and the coating. After the primer solidifies, the polyurea coating is sprayed with a coating thickness of 4 mm. After spraying, the sample is cured at room temperature for seven days and set aside.

[0071] Explosion test: The test was carried out in an explosion-proof pit. The explosive was a cylindrical column with a charge of 75g.

[0072] Shore hardness test: The coating was tested for hardness in accordance with the provisions of GB / T531.1-2008; the results are shown in Table 1.

[0073] Tensile strength, tear strength and elongation at break tests: refer to standard GB / T16777-2008 "Test methods for building waterproof coatings"; the results are shown in Table 1.

[0074] Cone calorimetry test: using the standard instrument of FTT Company of the United Kingdom, the sample size is 100mm×100mm×3mm, the radiation power is 5KW / m 2 .

[0075] Table 1

[0076]

[0077] Meanwhile, the contents not described in detail in this specification belong to the prior art known to those skilled in the art.

[0078] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0079] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A preparation process of a high-hardness polyurea coating anti-explosion coating material, characterized in that: The method comprises the following preparation steps: Step 1: Preheat the isocyanate prepolymer, amino-terminated polyether, chain extender, and additive in a drying oven at 75 to 80° C. for 45 to 60 minutes to ensure that the raw materials are in a liquid state; Step 2: After the preheating is completed, the amino-terminated polyether, the chain extender and the auxiliary agent are mixed evenly to obtain component A; Step 3: under the temperature condition of 50-70° C. and the pressure condition of 6-10 MPa, pour the isocyanate prepolymer into the A component, and mix and coat them to obtain the high-hardness polyurea coating anti-explosion coating material; The mass ratio of the isocyanate prepolymer to component A is (1-1.1):1; Among them, in parts by weight, the isocyanate prepolymer is 48 to 55 parts; in the A component, the amino-terminated polyether is 55 to 65 parts, the chain extender is 32 to 35 parts, and the auxiliary agent is 2.5 to 5 parts; The auxiliary agent comprises: 32wt%-40wt% of antifouling agent, 35wt%-46wt% of flame retardant, and 20wt%-32wt% of glass fiber.

2. The preparation process of the high-hardness polyurea coating explosion-proof coating material according to claim 1, characterized in that: The amino-terminated polyether is selected from one or more of secondary amino polyether diamines and secondary amino polyether triamines.

3. The preparation process of the high-hardness polyurea coating explosion-proof coating material according to claim 1, characterized in that: The -NCO content in the isocyanate prepolymer is 15.5 wt% to 17.5 wt%.

4. The preparation process of the high-hardness polyurea coating explosion-proof coating material according to claim 1, characterized in that: The chain extender is selected from one or more of 3,5-diethyltoluenediamine and 4,4-bis-sec-butylaminodiphenylmethane.

5. The preparation process of the high-hardness polyurea coating explosion-proof coating material according to claim 1, characterized in that: The preparation method of the antifouling agent is: 1) Pour 30 mL of dimethyl sulfoxide into 2,4,6-triaminopyrimidine and dissolve it while stirring; 2) At a temperature of 40-45°C, slowly add KH560 and react for 6-8 hours to obtain the antifouling agent.

6. The preparation process of the high-hardness polyurea coating explosion-proof coating material according to claim 5, characterized in that: In the antifouling agent, the weight proportions of the components added are: 25 to 35 parts of 2,4,6-triaminopyrimidine and 15 to 18 parts of KH560.

7. The preparation process of the high-hardness polyurea coating explosion-proof coating material according to claim 1, characterized in that: The specific preparation method of the flame retardant is: Ⅰ. Add 80 mL of distilled water to 0.6-1.5 parts of Zn(NO3)2·6H20 and stir at 350-400 rpm for 20-25 min. Ⅱ. Add 1.2-2.2 parts of NaOH, continue stirring for 15-20 minutes, place in a drying oven at 180-200°C for 18-24 hours, cool to room temperature, and then centrifuge at 6000-8000 rpm; Ⅲ. Pour 15-20 parts of solvent into a mixture of 0.08-0.1 parts of Co(NO3)2·6H20 and 2-3 parts of 2-methylimidazole. After dissolution, add 0.4-0.6 parts of the substance obtained in step Ⅱ and react at a temperature of 60-65°C for 1.5-2h. After the reaction is completed, cool to room temperature and wash with anhydrous ethanol and deionized water; IV. Then add 90-100 mL of 1,4-dioxane, perform ultrasonic dispersion, and then add 4,4'-diaminodiphenyl ether and hexachlorocyclotriphosphazene in sequence, stir at 75-80°C for 20-24 hours, cool to room temperature, and wash with anhydrous ethanol to obtain a flame retardant.

8. The process for preparing the high-hardness polyurea coating explosion-proof coating material according to claim 7, characterized in that: In the above III, the solvent is a mixed solution of dimethylformamide and distilled water, and the volume ratio thereof is 1:1.