Polyethylene terephthalate-based polyester fiber material and preparation method thereof

By connecting the two end crown ether modifications and amide ester of polyethylene terephthalate, a fiber material with a quasi-rotane structure is formed, which solves the problem of airtightness and difficulty in dyeing of the fiber material, and realizes thermal insulation and breathability and ease of use. The dyeing effect and improves hygroscopicity and antistatic properties.

CN118461177BActive Publication Date: 2024-11-05JIANGSU JIULINGWU NEW MATERIALS TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410909998.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-05
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

Polyethylene terephthalate fiber materials have problems such as airtightness and difficulty in dyeing in clothing applications, and the lack of hydrophilic groups leads to poor hygroscopicity.

Method used

Modified polyethylene terephthalate through the two-end crown ether modification and amide ester connection, forming a polyester fiber material with a quasi-rotane structure, using temperature changes to control the pores between polymer chains, increasing the hygroscopicity and flexibility of the material and easy dyeing is achieved through the destruction and formation of hydrogen bonds.

Benefits of technology

It realizes both thermal insulation and breathability of fiber materials and easy dyeing, improves moisture-absorbing and sweating properties and antistatic properties, and improves the dyeing properties of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118461177B_ABST
    Figure CN118461177B_ABST
Patent Text Reader

Abstract

The invention discloses a polyester fiber material based on polyethylene terephthalate and a preparation method thereof, belonging to the technical field of textile materials. Polyethylene terephthalate is modified to obtain polyethylene terephthalate modified with crown ethers at both ends and polyethylene terephthalate connected with amide esters, respectively. The action force between the crown ethers and the amides is used to form a pseudorotaxane structure, thereby increasing the sliding ability between polymer chains of the polyester fiber material, thereby controlling the pores between the polymer chains through temperature changes. Secondly, because the material has flexible ether chains and amide groups, it has the characteristics of moisture absorption and perspiration release, strong flexibility and antistatic properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of textile materials, and in particular relates to a polyester fiber material based on polyethylene terephthalate and a preparation method thereof. Background Art

[0002] Polyethylene terephthalate is a polyester polymer material with the characteristics of fineness, gloss, antistatic, water resistance, corrosion resistance, washability, and non-fading. In addition, the material has good processing properties and can be blended with various fibers to achieve different feel and fabric effects.

[0003] Polyethylene terephthalate has high heat resistance, thermal stability and softening point, so it has a good setting effect. However, polyethylene terephthalate lacks hydrophilic groups on the macromolecular chain, has a compact structure, small gaps between molecular chains, and low fiber hygroscopicity. Therefore, it has the advantages of easy washing and quick drying in clothing, but it also brings the disadvantage of clothing being airtight; because of the lack of polar groups in its chemical structure, it is difficult to combine with dyes, so generally under high temperature conditions, the thermal motion of the molecular chain segments is increased to increase the fiber micro-gap to achieve the purpose of dyeing. Therefore, how to modify it and prepare a polyester fiber material that is both heat-insulating and breathable and easy to dye while maintaining its excellent performance is of great significance. Summary of the invention

[0004] In order to solve the above problems, the object of the present invention is to provide a polyester fiber material based on polyethylene terephthalate and a preparation method thereof.

[0005] In order to achieve the above object, the present invention is implemented through the following technical solutions:

[0006] A polyester fiber material based on polyethylene terephthalate is composed of the following raw materials in parts by weight: 1 part of polyethylene terephthalate modified with crown ethers at both ends and 2-2.5 parts of polyethylene terephthalate connected with amide ester.

[0007] The polyethylene terephthalate modified with crown ethers at both ends is prepared according to the following method:

[0008] Add polyethylene terephthalate to dimethyl sulfoxide and concentrated sulfuric acid, then add dihydroxydibenzo-2,4-crown-8, grind and react at 25-30°C for 1-4 hours. After the reaction is completed, wash with tetrahydrofuran for 3-5 times to obtain polyethylene terephthalate modified with crown ethers at both ends.

[0009] The mass ratio of the polyethylene terephthalate, dimethyl sulfoxide, concentrated sulfuric acid and dihydroxydibenzo-2,4-crown-8 is 100:5-10:5-10:2-4.

[0010] The preparation method of the amide-ester-linked polyethylene terephthalate comprises the following steps:

[0011] (1) Add polyethylene terephthalate to a polar aprotic solvent, then add a catalyst and carbon tetrabromide thereto, react at 25-30°C for 1.5-2.5 hours, remove the solvent by vacuum distillation, add the resulting residue to an alcohol solvent, then add hydrazine hydrate thereto, boil and stir to react for 10-30 minutes, filter, and wash the resulting filter cake alternately with water and an organic solvent to obtain a solid;

[0012] (2) The solid obtained in step (1) is divided into two equal parts, a polar aprotic solvent and triphosgene are added to one part, and the mixture is stirred for reaction for 1 hour, and then the other part of the solid and dibutyltin dilaurate are added, and the mixture is stirred for reaction for 0.5 to 1 hour. The solvent is removed by vacuum distillation, and the residue is washed alternately with water and an organic solvent to obtain amide-ester-linked polyethylene terephthalate.

[0013] The polar aprotic solvent is dimethyl sulfoxide, dimethylformamide or N-methylpyrrolidone.

[0014] The catalyst is triphenylphosphine or tributylphosphine.

[0015] The mass ratio of polyethylene terephthalate, polar aprotic solvent, catalyst, carbon tetrabromide, alcohol solvent and hydrazine hydrate in step (1) is 1:10-20:2-2.5:1-1.5:5-10:2-3.

[0016] The alcohol solvent is methanol, ethanol or isopropanol.

[0017] The organic solvent is ethanol, acetone, methanol or acetonitrile.

[0018] The mass ratio of the polar aprotic solvent, triphosgene, dibutyltin dilaurate in step (2) to the polyethylene terephthalate in step (1) is 5-10:1-1.2:0.05-0.1:1.

[0019] The method for preparing the polyester fiber material based on polyethylene terephthalate comprises mixing, by weight, 1 part of polyethylene terephthalate modified with crown ethers at both ends and 2 to 2.5 parts of polyethylene terephthalate connected with amide esters, heating to 200 to 220° C. for melting, stirring for 20 to 40 minutes, and finally spinning to prepare the polyester fiber material based on polyethylene terephthalate.

[0020] Compared with the prior art, the present invention has the following advantages:

[0021] The polyester fiber material based on polyethylene terephthalate of the present invention is prepared by modifying polyethylene terephthalate to obtain polyethylene terephthalate modified with crown ethers at both ends and polyethylene terephthalate connected by amide esters, and the interaction between the crown ethers and the amides is used to form a pseudorotaxane structure, thereby increasing the sliding ability between polymer chains of the polyester fiber material, thereby controlling the pores between the polymer chains through temperature changes; secondly, because it has flexible ether chains and amide groups, the material has the characteristics of moisture absorption and perspiration release, strong flexibility and antistatic properties.

[0022] The polyester fiber material based on polyethylene terephthalate of the present invention utilizes the motion characteristics of the pseudorotaxane structure. When the temperature is high, the polymer chain segment macromolecular motion is intensified, the hydrogen bonds between the macromolecular chain segments are destroyed, and the rotaxane structure is in a stretched state; when the temperature is low, the hydrogen bonds between two adjacent polymer chains in the rotaxane structure are strengthened, and the rotaxane is in a contracted state. The schematic diagram of the movement of the rotaxane structure when the temperature changes is shown in FIG. Figure 1 As shown; therefore, the prepared material achieves the purpose of being easy to dye. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a schematic diagram of the structural movement of the polyester fiber material of the present invention when the temperature changes. DETAILED DESCRIPTION

[0024] In order to better understand the technical solution of the present invention, the above content of the present invention is further described in detail below through specific implementation methods in the form of embodiments, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples. All technologies realized based on the above content of the present invention belong to the scope of the present invention.

[0025] Example 1 Preparation of polyethylene terephthalate modified with crown ethers at both ends:

[0026] 1 kg of polyethylene terephthalate was added to 0.05 kg of dimethyl sulfoxide and 0.05 kg of concentrated sulfuric acid, and then 0.02 kg of dihydroxydibenzo-2,4-crown-8 was added thereto. The mixture was ground and reacted at 25°C for 1 hour. After the reaction was completed, the mixture was washed with tetrahydrofuran for 3 times to obtain polyethylene terephthalate modified with crown ethers at both ends.

[0027] Preparation of amide-ester linked polyethylene terephthalate:

[0028] (1) Add 0.1 kg of polyethylene terephthalate to 1 kg of dimethyl sulfoxide, then add 0.2 kg of triphenylphosphine and 0.1 kg of carbon tetrabromide, react at 25°C for 1.5 hours, remove the solvent by distillation under reduced pressure, add the residue to 0.5 kg of methanol, then add 0.2 kg of hydrazine hydrate, boil and stir to react for 10 minutes, filter, and wash the filter cake alternately with water and ethanol to obtain a solid;

[0029] (3) The obtained solid was divided into two equal parts, 0.5 kg of dimethyl sulfoxide and 0.1 kg of triphosgene were added to one part, and the mixture was stirred for reaction for 1 hour. Then, the other part of the solid and 0.005 kg of dibutyltin dilaurate were added, and the mixture was stirred for reaction for 0.5 hour. The solvent was removed by distillation under reduced pressure, and the obtained residue was washed alternately with water and ethanol to obtain amide-ester-linked polyethylene terephthalate.

[0030] Preparation of polyester fiber materials based on polyethylene terephthalate:

[0031] 1 kg of polyethylene terephthalate modified with crown ethers at both ends and 2 kg of polyethylene terephthalate connected with amide ester were mixed, heated to 200° C. for melting, stirred for 20 minutes, and finally spun to prepare a polyester fiber material based on polyethylene terephthalate.

[0032] Example 2 Preparation of polyethylene terephthalate modified with crown ethers at both ends:

[0033] 1 kg of polyethylene terephthalate was added to 0.06 kg of dimethyl sulfoxide and 0.06 kg of concentrated sulfuric acid, and then 0.025 kg of dihydroxydibenzo-2,4-crown-8 was added thereto. The mixture was ground and reacted at 26°C for 1.5 hours. After the reaction was completed, it was washed with tetrahydrofuran for 3 times to obtain polyethylene terephthalate modified with crown ethers at both ends.

[0034] Preparation of amide-ester linked polyethylene terephthalate:

[0035] (1) Add 0.1 kg of polyethylene terephthalate to 1.2 kg of dimethylformamide, then add 0.21 kg of tributylphosphine and 0.11 kg of carbon tetrabromide, react at 28°C for 1.8 hours, remove the solvent by distillation under reduced pressure, add the residue to 0.6 kg of ethanol, then add 0.22 kg of hydrazine hydrate, boil and stir to react for 15 minutes, filter, and wash the filter cake alternately with water and acetone to obtain a solid;

[0036] (3) The obtained solid was divided into two equal parts, 0.6 kg of dimethyl sulfoxide and 0.11 kg of triphosgene were added to one part, and the mixture was stirred for reaction for 1 hour. Then, the other part of the solid and 0.006 kg of dibutyltin dilaurate were added, and the mixture was stirred for reaction for 0.6 hour. The solvent was removed by distillation under reduced pressure, and the obtained residue was washed alternately with water and methanol to obtain amide-ester-linked polyethylene terephthalate.

[0037] Preparation of polyester fiber materials based on polyethylene terephthalate:

[0038] 1 kg of polyethylene terephthalate modified with crown ethers at both ends and 2.1 kg of polyethylene terephthalate connected with amide ester were mixed, heated to 210° C. for melting, stirred for 25 minutes, and finally spun to prepare a polyester fiber material based on polyethylene terephthalate.

[0039] Example 3 Preparation of polyethylene terephthalate modified with crown ethers at both ends:

[0040] 1 kg of polyethylene terephthalate was added to 0.075 kg of dimethyl sulfoxide and 0.07 kg of concentrated sulfuric acid, and then 0.03 kg of dihydroxydibenzo-2,4-crown-8 was added thereto. The mixture was ground and reacted at 28°C for 2 hours. After the reaction was completed, it was washed with tetrahydrofuran for 4 times to obtain polyethylene terephthalate modified with crown ethers at both ends.

[0041] Preparation of amide-ester linked polyethylene terephthalate:

[0042] (1) 0.1 kg of polyethylene terephthalate was added to 1.4 kg of N-methylpyrrolidone, and then 0.22 kg of tributylphosphine and 0.12 kg of carbon tetrabromide were added thereto. The mixture was reacted at 30°C for 2 h. The solvent was removed by distillation under reduced pressure. The residue was added to 0.7 kg of isopropanol, and then 0.24 kg of hydrazine hydrate was added thereto. The mixture was stirred and boiled for 20 min. The mixture was filtered and the filter cake was washed alternately with water and methanol to obtain a solid.

[0043] (3) The obtained solid was divided into two equal parts, 0.7 kg of dimethyl sulfoxide and 0.11 kg of triphosgene were added to one part, and the mixture was stirred for reaction for 1 hour. Then, the other part of the solid and 0.007 kg of dibutyltin dilaurate were added, and the mixture was stirred for reaction for 0.7 hour. The solvent was removed by distillation under reduced pressure, and the obtained residue was washed alternately with water and acetone to obtain amide-ester-linked polyethylene terephthalate.

[0044] Preparation of polyester fiber materials based on polyethylene terephthalate:

[0045] 1 kg of polyethylene terephthalate modified with crown ethers at both ends and 2.2 kg of polyethylene terephthalate connected with amide ester were mixed, heated to 205° C. for melting, stirred for 30 minutes, and finally spun to prepare a polyester fiber material based on polyethylene terephthalate.

[0046] Example 4 Preparation of polyethylene terephthalate modified with crown ethers at both ends:

[0047] 1 kg of polyethylene terephthalate was added to 0.08 kg of dimethyl sulfoxide and 0.07 kg of concentrated sulfuric acid, and then 0.035 kg of dihydroxydibenzo-2,4-crown-8 was added thereto. The mixture was ground and reacted at 29°C for 2.5 hours. After the reaction was completed, the mixture was washed with tetrahydrofuran for 4 times to obtain polyethylene terephthalate modified with crown ethers at both ends.

[0048] Preparation of amide-ester linked polyethylene terephthalate:

[0049] (1) Add 0.1 kg of polyethylene terephthalate to 1.6 kg of dimethyl sulfoxide, then add 0.23 kg of triphenylphosphine and 0.13 kg of carbon tetrabromide, react at 28°C for 2.2 hours, remove the solvent by distillation under reduced pressure, add the residue to 0.75 kg of methanol, then add 0.26 kg of hydrazine hydrate, boil and stir to react for 25 minutes, filter, and wash the filter cake alternately with water and acetonitrile to obtain a solid;

[0050] (3) The obtained solid was divided into two equal parts, 0.75 kg of dimethylformamide and 0.11 kg of triphosgene were added to one part, and the mixture was stirred for reaction for 1 hour. Then, the other part of the solid and 0.008 kg of dibutyltin dilaurate were added, and the mixture was stirred for reaction for 0.8 hour. The solvent was removed by distillation under reduced pressure, and the obtained residue was washed alternately with water and acetonitrile to obtain amide-ester-linked polyethylene terephthalate.

[0051] Preparation of polyester fiber materials based on polyethylene terephthalate:

[0052] 1 kg of polyethylene terephthalate modified with crown ethers at both ends and 2.3 kg of polyethylene terephthalate connected with amide ester were mixed, heated to 210° C. for melting, stirred for 30 minutes, and finally spun to prepare a polyester fiber material based on polyethylene terephthalate.

[0053] Example 5 Preparation of polyethylene terephthalate modified with crown ethers at both ends:

[0054] 1 kg of polyethylene terephthalate was added to 0.1 kg of dimethyl sulfoxide and 0.1 kg of concentrated sulfuric acid, and then 0.04 kg of dihydroxydibenzo-2,4-crown-8 was added thereto. The mixture was ground and reacted at 30°C for 4 hours. After the reaction was completed, it was washed with tetrahydrofuran for 5 times to obtain polyethylene terephthalate modified with crown ethers at both ends.

[0055] Preparation of amide-ester linked polyethylene terephthalate:

[0056] (1) Add 0.1 kg of polyethylene terephthalate to 2 kg of dimethyl sulfoxide, then add 0.25 kg of triphenylphosphine and 0.15 kg of carbon tetrabromide, react at 30°C for 2.5 hours, remove the solvent by distillation under reduced pressure, add the residue to 1 kg of isopropanol, then add 0.3 kg of hydrazine hydrate, boil and stir to react for 30 minutes, filter, and wash the filter cake alternately with water and ethanol to obtain a solid;

[0057] (3) The obtained solid was divided into two equal parts. 1 kg of N-methylpyrrolidone and 0.12 kg of triphosgene were added to one part. After stirring for 1 hour, the other part of the solid and 0.01 kg of dibutyltin dilaurate were added. After stirring for 1 hour, the solvent was removed by distillation under reduced pressure. The obtained residue was washed alternately with water and acetonitrile to obtain amide-ester-linked polyethylene terephthalate.

[0058] Preparation of polyester fiber materials based on polyethylene terephthalate:

[0059] 1 kg of polyethylene terephthalate modified with crown ethers at both ends and 2.5 kg of polyethylene terephthalate connected with amide ester were mixed, heated to 220° C. for melting, stirred for 40 minutes, and finally spun to prepare a polyester fiber material based on polyethylene terephthalate.

[0060] Example 6 Preparation of polyethylene terephthalate modified with crown ethers at both ends:

[0061] 1 kg of polyethylene terephthalate was added to 0.05 kg of dimethyl sulfoxide and 0.1 kg of concentrated sulfuric acid, and then 0.03 kg of dihydroxydibenzo-2,4-crown-8 was added thereto. The mixture was ground and reacted at 30°C for 1 hour. After the reaction was completed, the mixture was washed with tetrahydrofuran for 5 times to obtain polyethylene terephthalate modified with crown ethers at both ends.

[0062] Preparation of amide-ester linked polyethylene terephthalate:

[0063] (1) Add 0.1 kg of polyethylene terephthalate to 1.2 kg of dimethyl sulfoxide, then add 0.25 kg of triphenylphosphine and 0.1 kg of carbon tetrabromide, react at 25°C for 2.5 hours, remove the solvent by distillation under reduced pressure, add the residue to 0.8 kg of isopropanol, then add 0.25 kg of hydrazine hydrate, boil and stir to react for 10 minutes, filter, and wash the filter cake alternately with water and acetonitrile to obtain a solid;

[0064] (3) The obtained solid was divided into two equal parts, 0.8 kg of dimethylformamide and 0.12 kg of triphosgene were added to one part, and the mixture was stirred for reaction for 1 hour. Then, the other part of the solid and 0.005 kg of dibutyltin dilaurate were added, and the mixture was stirred for reaction for 0.5 hour. The solvent was removed by distillation under reduced pressure, and the obtained residue was washed alternately with water and acetonitrile to obtain amide-ester-linked polyethylene terephthalate.

[0065] Preparation of polyester fiber materials based on polyethylene terephthalate:

[0066] 1 kg of polyethylene terephthalate modified with crown ethers at both ends and 2.3 kg of polyethylene terephthalate connected with amide ester were mixed, heated to 220° C. for melting, stirred for 20 minutes, and finally spun to prepare a polyester fiber material based on polyethylene terephthalate.

[0067] Comparative Example: Polyethylene terephthalate was heated to 300° C. to melt, and finally spun to obtain a polyester fiber material.

[0068] The polyethylene terephthalate-based polyester fiber materials prepared in Examples 1 to 6 and the polyester fiber material prepared in the comparative example were tested respectively, and the test results are shown in Table 1.

[0069] Table 1 Performance parameters of polyester fiber materials prepared in Examples 1 to 6

[0070]

[0071] It can be seen from the results in Table 1 that the polyester fiber material based on polyethylene terephthalate of the present invention has a higher moisture regain, a lower contact angle, and an initial modulus lower than that of the polyester fiber material prepared from unmodified polyethylene terephthalate, indicating that the material of the present invention has better hygroscopicity and strong softness.

[0072] Although the above describes the specific implementation methods of the present invention, it does not limit the scope of protection of the present invention. Based on the technical solution of the present invention, various modifications or variations that can be made by those skilled in the art without creative work are still within the scope of protection of the present invention.

Claims

1. A polyester fiber material based on polyethylene terephthalate, characterized in that: The invention is composed of the following raw materials in parts by weight: 1 part of polyethylene terephthalate modified with crown ethers at both ends and 2-2.5 parts of polyethylene terephthalate connected with amide ester; The polyethylene terephthalate modified with crown ethers at both ends is prepared according to the following method: Add polyethylene terephthalate to dimethyl sulfoxide and concentrated sulfuric acid, then add dihydroxydibenzo-24-crown-8, grind and react at 25-30°C for 1-4 hours, and after the reaction is completed, wash with tetrahydrofuran 3-5 times to obtain polyethylene terephthalate modified with crown ethers at both ends; The mass ratio of polyethylene terephthalate, dimethyl sulfoxide, concentrated sulfuric acid and dihydroxydibenzo-24-crown-8 is 100:5-10:5-10:2-4; The preparation method of the amide-ester-linked polyethylene terephthalate comprises the following steps: (1) Add polyethylene terephthalate to a polar aprotic solvent, then add a catalyst and carbon tetrabromide thereto, react at 25-30°C for 1.5-2.5 hours, remove the solvent by vacuum distillation, add the resulting residue to an alcohol solvent, then add hydrazine hydrate thereto, boil and stir to react for 10-30 minutes, filter, and wash the resulting filter cake alternately with water and an organic solvent to obtain a solid; (2) The solid obtained in step (1) is divided into two equal parts, a polar aprotic solvent and triphosgene are added to one part, and the mixture is stirred for reaction for 1 hour, and then the other part of the solid and dibutyltin dilaurate are added, and the mixture is stirred for reaction for 0.5 to 1 hour. The solvent is removed by vacuum distillation, and the residue is washed alternately with water and an organic solvent to obtain amide-ester-linked polyethylene terephthalate; The mass ratio of polyethylene terephthalate, polar aprotic solvent, catalyst, carbon tetrabromide, alcohol solvent and hydrazine hydrate in step (1) is 1:10-20:2-2.5:1-1.5:5-10:2-3; The mass ratio of the polar aprotic solvent, triphosgene, dibutyltin dilaurate and the polyethylene terephthalate in step (2) is 5-10:1-1.2:0.05-0.1:1; The polyethylene terephthalate modified with crown ethers at both ends and the polyethylene terephthalate connected with amide ester are mixed, heated to melt, stirred, and spun to prepare a polyester fiber material based on polyethylene terephthalate.

2. The polyester fiber material based on polyethylene terephthalate according to claim 1, characterized in that: The polar aprotic solvent is dimethyl sulfoxide, dimethylformamide or N-methylpyrrolidone.

3. The polyethylene terephthalate-based polyester fiber material according to claim 1, characterized in that: The catalyst is triphenylphosphine or tributylphosphine.

4. The polyethylene terephthalate-based polyester fiber material according to claim 1, characterized in that: The alcohol solvent is methanol, ethanol or isopropanol; the organic solvent is ethanol, acetone, methanol or acetonitrile.

5. The method for preparing the polyester fiber material based on polyethylene terephthalate according to claim 1, characterized in that: In parts by weight, 1 part of polyethylene terephthalate modified with crown ethers at both ends and 2-2.5 parts of polyethylene terephthalate connected with amide esters are mixed, heated to 200-220° C. for melting, stirred for 20-40 minutes, and finally spun to prepare a polyester fiber material based on polyethylene terephthalate.