Vinyl silane modified core-shell structure composite material and its application in railway deicing

The core-shell structure composite material modified by vinyl silane, combined with rare earth hexaboride and super-hydrophobic vinyl-modified silica, solves the problems of environmentally harmful fluorine materials and insufficient hydrophobicity of silica in the existing technology. , achieving efficient anti-icing and rapid ice melting, protecting the environment and reducing costs.

CN118480331BActive Publication Date: 2024-10-18TIANJIN BAOGANG RES INST OF RARE EARTHS CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410946448.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-18
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

Among the existing anti-icing technologies, fluorine-containing materials are harmful to the environment and are costly. The hydrophobicity of silica cannot completely prevent the formation of ice. In particular, the problem of rapid condensation of ice during high-speed rail operation is difficult to solve.

Method used

Using vinyl silane-modified core-shell structure composite materials, through the photothermal effect of rare earth hexaboride and super-hydrophobic vinyl-modified silica, combined with core-shell structure technology, it forms an anti-static material with rapid heat absorption and high hydrophobicity. Ice material.

Benefits of technology

It can effectively prevent the formation of ice and quickly melt ice during high-speed rail operation, protecting the environment, and the hydrophobicity and heat absorption of the material have been significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118480331B_ABST
    Figure CN118480331B_ABST
Patent Text Reader

Abstract

The present invention provides a composite material of a core-shell structure modified by vinyl silane and its application in railway deicing, wherein the composite material is prepared by raw materials including the following mass fractions: 0.23-0.57 parts of rare earth hexaboride; 26.30-31.20 parts of alkaline catalyst; 0.27-0.33 parts of silicon source; 66.36-72.56 parts of ethanol; 0.60-0.89 parts of vinyl silane modifier; the sum of the mass fractions of each component is 100 parts. The present invention utilizes rare earth materials that can have rapid heat absorption characteristics to provide a huge effect in ice melting. While the core-shell structure is used to protect the internal rare earth boride from being destroyed, the shell in the present invention adopts vinyl modified silica with super hydrophobic properties, and the modified material has a stronger hydrophobic property than silica, which can achieve rapid ice melting while effectively preventing ice.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of railway anti-icing and deicing, and in particular relates to a vinyl silane-modified core-shell structure composite material and its application in railway deicing. Background Art

[0002] Existing anti-icing technologies usually use hydrophobic resins made of low surface energy composite materials such as silica and fluorine, but these composite resins are very harmful to the environment and have varying degrees of irritation to human skin and mucous membranes. The previously reported article "Preparation and Performance Study of Anti-icing Hydrophobic Coatings Based on Nano-Silica" discloses a self-assembled nano-silica / fluorosilicone resin-epoxy resin composite hydrophobic coating modified by HTPS (terminated hydroxyl polydimethylsiloxane) and APTES (aminopropyltriethoxysilane). Although fluorine-based resins or modified materials are not good for the environment, silica is often used in anti-icing materials due to its excellent hydrophobic and dispersible properties.

[0003] At present, most existing technologies use the hydrophobic properties of fluorine-containing hydrophobic materials to prevent ice from sticking to the iron plate. However, fluorine-containing substances are extremely harmful to the environment and are expensive. As for hydrophobic materials such as silicon dioxide, for high-speed trains in rapid motion, ice is formed not only by water solidifying into ice, but also by water vapor directly condensing into ice. The hydrophobicity of silicon dioxide itself cannot completely prevent the formation of ice. Summary of the invention

[0004] In view of this, the present invention aims to overcome the defects in the prior art and proposes a vinyl silane-modified core-shell structure composite material and its application in railway deicing.

[0005] To achieve the above object, the technical solution of the present invention is achieved as follows:

[0006] In a first aspect of the present invention, there is provided a vinyl silane-modified core-shell structure composite material, wherein the composite material is prepared from raw materials comprising the following weight fractions:

[0007] Rare earth hexaboride 0.23-0.57 parts;

[0008] 26.3-31.2 parts of basic catalyst;

[0009] Silicon source 0.27-0.33 parts;

[0010] Ethanol 66.36-72.56 parts;

[0011] Vinyl silane modifier 0.60-0.89 parts.

[0012] Preferably, the rare earth hexaboride is one or more of LaB6, SmB6, and CeB6.

[0013] Preferably, the alkaline catalyst is one or more of sodium hydroxide, ammonia water and triethylamine.

[0014] Preferably, the silicon source is one or more of tetraethyl orthosilicate, methyltrimethoxysilane, and ammonium hexafluorosilicate.

[0015] Preferably, the vinyl silane modifier is one or more of vinyl triethoxysilane, vinyl triisopropoxysilane, and vinyl tributylidene oxime silane.

[0016] Among the above raw materials:

[0017] The rare earth hexaboride is a rare earth nanoparticle with photothermal effect, which is placed inside the core-shell structure as an important substance for absorbing heat and melting ice.

[0018] The alkaline catalyst is used to create an alkaline environment, which is beneficial to the etching of the three-dimensional structure and the preparation of the core-shell structure.

[0019] The silicon source is a raw material for preparing the core-shell structure ReB6@SiO2, which has low volatility and good solubility. It can undergo a core-shell reaction under the promotion of ethanol, and after the reaction it becomes a shell with functional groups, which can not only protect the internal rare earth hexaboride from corrosion but also modify other functional groups on its surface to meet specific applications.

[0020] The ethanol is not only a reaction solvent for preparing the core-shell structure ReB6@SiO2, but also a reaction solvent for the next step modification reaction of the core-shell nanoparticles and vinyltriethoxysilane.

[0021] The vinyl silane modifier is a modifier that uses its unique excellent hydrophobic properties to treat nano silicon dioxide particles. The obtained vinyl modified silicon dioxide has better super hydrophobic properties than silicon dioxide, and the reaction byproducts are non-corrosive, which is beneficial to protecting equipment and the environment and creating an alkaline environment.

[0022] More preferably, the rare earth hexaboride is LaB6; the alkaline catalyst is ammonia water; the silicon source is tetraethyl orthosilicate; and the vinyl silane modifier is vinyl triethoxysilane. In this case, the composite material of the present invention is LaB6@SiO2, and its synthesis route is:

[0023]

[0024] The second aspect of the present invention further provides a method for preparing the above-mentioned vinyl silane-modified core-shell structure composite material, the preparation method comprising the following steps:

[0025] 1) Mixing rare earth hexaboride and ethanol and ultrasonically dispersing for 1-3 hours to obtain a mixed solution;

[0026] 2) Add alkaline catalyst and silicon source to the mixed solution, stir at room temperature for 2-3 hours, and then centrifuge and wash to obtain core-shell structure ReB6@SiO2;

[0027] 3) The core-shell structure ReB6@SiO2 is dispersed in ethanol, an alkaline catalyst is added to adjust to neutrality, and then a vinyl silane modifier is added. After stirring at 55-65°C for 18-24h, the vinyl silane-modified core-shell structure ReB6@SiO2 is obtained by filtering, washing and drying.

[0028] The third aspect of the present invention also provides the use of the above-mentioned vinyl silane-modified core-shell structure composite material in the preparation of an anti-icing and de-icing agent.

[0029] The fourth aspect of the present invention also provides the use of the above-mentioned vinyl silane-modified core-shell structure composite material in the preparation of railway deicing products.

[0030] Compared with the prior art, the present invention has the following advantages:

[0031] (1) The present invention provides a core-shell structure of vinyl silane-modified silica coated with rare earth hexaboride. In terms of heat absorption and ice melting, rare earth hexaboride is a rare earth material with excellent photothermal conversion efficiency, which can achieve rapid temperature rise in a short time. However, using ice melting alone cannot solve the problem of large amounts of ice and rapid condensation during high-speed rail operation. Therefore, in terms of ice prevention, the present invention adds vinyl-modified silica with super-hydrophobic properties on the basis of heat absorption, and wraps it as a shell on the surface of inorganic rare earth particles. On the one hand, it protects the inorganic material so that it will not be damaged under repeated use conditions, and on the other hand, it increases the coverage area of ​​the hydrophobic material, which has a significant effect in ice prevention.

[0032] (2) The present invention utilizes rare earth materials that have the property of rapid heat absorption to provide a great effect in melting ice. While using the core-shell structure to protect the rare earth boride inside from being destroyed, the shell of the present invention uses vinyl-modified silica with super-hydrophobic properties. The modified material has a stronger hydrophobic property than silica, and can effectively prevent ice while achieving rapid ice melting.

[0033] (3) Compared with the traditional hydrophobic silica material, the present invention has a stronger hydrophobicity than silica by grafting hydrophobic groups on the surface of the silica shell. Compared with fluorine-containing resins, the hydrophobic material used in the present invention protects the environment without affecting its hydrophobic properties. In addition, the core-shell structure is used to coat the silica on the outside of the rare earth nanoparticles, which protects the surface of the rare earth particles from being adhered by the ice layer and does not affect the heat absorption characteristics of the rare earth nanoparticles.

[0034] (4) The hydrophobicity of the present invention was characterized by water contact angle test, which confirmed that the super-hydrophobic surface after vinyl modification has higher hydrophobicity than silica. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a transmission electron microscope image of the vinyl silane-modified core-shell structure composite material LaB6@SiO2 prepared in Example 1;

[0036] Figure 2 This is a water contact angle diagram of the core-shell structure composite material coating modified by vinyl silane prepared in Example 1;

[0037] Figure 3 This is a water contact angle diagram of the silicon dioxide coating prepared in Comparative Example 1;

[0038] Figure 4 This is a comparison chart of ice melting rates of Examples 1-5;

[0039] Figure 5 The ice melting rate curves of Example 1 and Comparative Examples 1-5 are shown. DETAILED DESCRIPTION

[0040] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.

[0041] The present invention will be described in detail below with reference to the embodiments.

[0042] Example 1

[0043] A method for preparing a vinylsilane-modified core-shell structure composite material LaB6@SiO2 comprises the following steps:

[0044] 1) Add LaB6 (2.04 g, 10.00 mmol) and ethanol (200 mL) into a 500 mL beaker and disperse under ultrasound for 1 h.

[0045] 2) Add ammonia water (50 mL) and tetraethyl orthosilicate (1.02 g, 4.90 mmol) to the dispersed solution, stir at room temperature for 2 h, and then centrifuge and wash to obtain the core-shell structure LaB6@SiO2.

[0046] 3) The washed product was dispersed in ethanol (100 mL), and ammonia water (75 mL) was added to adjust to neutrality, followed by vinyltriethoxysilane (3.16 g, 16.60 mmol). The mixture was placed in a 60°C oil bath and stirred for 20 h. The mixture was cooled to room temperature and filtered. The mixture was washed with ethanol and dried in a 70°C vacuum oven for 12 h to obtain a vinylsilane-modified core-shell composite material LaB6@SiO2.

[0047] Example 2

[0048] A method for preparing a vinylsilane-modified core-shell structure composite material LaB6@SiO2 comprises the following steps:

[0049] 1) Add LaB6 (2.04 g, 10.00 mmol) and ethanol (500 mL) into a 500 mL beaker and disperse under ultrasound for 1 h.

[0050] 2) Add ammonia water (100 mL) and tetraethyl orthosilicate (2.09 g, 10.00 mmol) to the dispersed solution, stir at room temperature for 2 h, and then centrifuge and wash to obtain the core-shell structure LaB6@SiO2.

[0051] 3) The washed product was dispersed in ethanol (200 mL), and ammonia water (120 mL) was added to adjust to neutrality, followed by vinyltriethoxysilane (4.52 g, 23.75 mmol). The mixture was placed in a 60°C oil bath and stirred for 20 h. The mixture was cooled to room temperature and filtered. The mixture was washed with ethanol and dried in a 70°C vacuum oven for 12 h to obtain a vinylsilane-modified core-shell composite material LaB6@SiO2.

[0052] Example 3

[0053] A method for preparing a vinylsilane-modified core-shell structure composite material LaB6@SiO2 comprises the following steps:

[0054] 1) Add LaB6 (2.04 g, 10.00 mmol) and ethanol (520 mL) into a 500 mL beaker and disperse under ultrasound for 1 h.

[0055] 2) Add ammonia water (120 mL) and tetraethyl orthosilicate (3.06 g, 14.69 mmol) to the dispersed solution, stir at room temperature for 2 h, and then centrifuge and wash to obtain the core-shell structure LaB6@SiO2.

[0056] 3) The washed product was dispersed in ethanol (230 mL), and ammonia water (180 mL) was added to adjust to neutrality, followed by vinyltriethoxysilane (5.24 g, 27.53 mmol). The mixture was placed in a 60°C oil bath and stirred for 20 h. The mixture was cooled to room temperature and filtered. The mixture was washed with ethanol and dried in a 70°C vacuum oven for 12 h to obtain a vinylsilane-modified core-shell composite material LaB6@SiO2.

[0057] Example 4

[0058] A method for preparing a vinylsilane-modified core-shell structure composite material SmB6@SiO2 comprises the following steps:

[0059] 1) SmB6 (2.04 g, 10.01 mmol) and ethanol (500 mL) were added to a 500 mL beaker and dispersed under ultrasound for 3 h.

[0060] 2) Add sodium hydroxide (110 g, 2.75 mol) and methyltrimethoxysilane (3.00 g, 22.02 mmol) to the dispersed solution, stir at room temperature for 3 h, and then centrifuge and wash to obtain the core-shell structure SmB6@SiO2.

[0061] 3) The washed product was dispersed in ethanol (230 mL), sodium hydroxide (160 g, 4.00 mol) was added to adjust to neutrality, and then vinyl triisopropoxy silane (5.00 g, 21.52 mmol) was added. After being placed in a 65°C oil bath and stirred for 24 h, the mixture was cooled to room temperature and filtered. The mixture was washed with ethanol and dried in a 70°C vacuum oven for 12 h to obtain a vinyl silane-modified core-shell composite material SmB6@SiO2.

[0062] Example 5

[0063] A method for preparing a vinylsilane-modified core-shell composite material CeB6@SiO2 comprises the following steps:

[0064] 1) Add SmB6 (2.04 g, 10.01 mmol) and ethanol (500 mL) into a 500 mL beaker and disperse under ultrasound for 1 h.

[0065] 2) Add triethylamine (140 mL) and ammonium hexafluorosilicate (3.00 g, 16.84 mmol) to the dispersed solution, stir at room temperature for 2 h, and then centrifuge and wash to obtain the core-shell structure CeB6@SiO2.

[0066] 3) The washed product was dispersed in ethanol (230 mL), triethylamine (210 mL) was added to adjust to neutrality, and then vinyltributylidene silane (5.00 g, 15.95 mmol) was added. After being placed in a 55°C oil bath and stirred for 18 h, the mixture was cooled to room temperature and filtered. The mixture was washed with ethanol and dried in a 70°C vacuum oven for 12 h to obtain a vinylsilane-modified core-shell composite material CeB6@SiO2.

[0067] Comparative Example 1:

[0068] This comparative example provides a method for preparing a vinyl silane-modified core-shell structure composite material GdB6@SiO2, which differs from Example 1 in that: in step 1), GdB6 is added into a beaker, and the other steps, raw materials and proportions are the same as those in Example 1.

[0069] Comparative Example 2:

[0070] This comparative example provides a method for preparing a vinylsilane-modified core-shell structure composite material La2O3@SiO2, which differs from Example 1 in that: in step 1), La2O3 is added into a beaker, and the other steps, raw materials and proportions are the same as those in Example 1.

[0071] Comparative Example 3:

[0072] A method for preparing a vinylsilane-modified core-shell structure composite material LaB6@SiO2 comprises the following steps:

[0073] 1) Add LaB6 (1.02 g, 5.00 mmol) and ethanol (200 mL) into a 500 mL beaker and disperse under ultrasound for 1 h.

[0074] 2) Add ammonia water (50 mL) and tetraethyl orthosilicate (1.02 g, 4.90 mmol) to the dispersed solution, stir at room temperature for 2 h, and then centrifuge and wash to obtain the core-shell structure LaB6@SiO2.

[0075] 3) The washed product was dispersed in ethanol (100 mL), and ammonia water (75 mL) was added to adjust to neutrality, followed by vinyltriethoxysilane (3.16 g, 16.60 mmol). The mixture was placed in a 60°C oil bath and stirred for 20 h. The mixture was cooled to room temperature and filtered. The mixture was washed with ethanol and dried in a 70°C vacuum oven for 12 h to obtain a vinylsilane-modified core-shell composite material LaB6@SiO2.

[0076] Comparative Example 4:

[0077] A method for preparing a vinylsilane-modified core-shell structure composite material LaB6@SiO2 comprises the following steps:

[0078] 1) Add LaB6 (4.08 g, 20.00 mmol) and ethanol (200 mL) into a 500 mL beaker and disperse under ultrasound for 1 h.

[0079] 2) Add ammonia water (50 mL) and tetraethyl orthosilicate (1.02 g, 4.90 mmol) to the dispersed solution, stir at room temperature for 2 h, and then centrifuge and wash to obtain the core-shell structure LaB6@SiO2.

[0080] 3) The washed product was dispersed in ethanol (100 mL), and ammonia water (75 mL) was added to adjust to neutrality, followed by vinyltriethoxysilane (3.16 g, 16.60 mmol). The mixture was placed in a 60°C oil bath and stirred for 20 h. The mixture was cooled to room temperature and filtered. The mixture was washed with ethanol and dried in a 70°C vacuum oven for 12 h to obtain a vinylsilane-modified core-shell composite material LaB6@SiO2.

[0081] Comparative Example 5:

[0082] 1) Using anhydrous ethanol as a dispersant and an ammonia solution as a catalyst, nano-silica particles were prepared by hydrolyzing tetraethoxysilane. The mixture was stirred at room temperature for 24 hours, centrifuged, washed with anhydrous ethanol three times, and then vacuum dried for 12 hours.

[0083] 2) 3 g of nano-silicon dioxide particles were placed in 25 mL of hexanol and ultrasonically dispersed for 20 min. The above mixture was first mixed with 1 g of HTPS (high temperature polycrystalline silicon) and stirred at room temperature for 24 h, then mixed with 0.08 g of DBTD (dibutyltin dilaurate) and 10 mL of hexanol and stirred for 30 min, and then dried at 60 °C for 2 h.

[0084] 3) Disperse 3 g of HTPS-modified nano-silica particles and 1 mL of APTES (aminosilane) in 30 mL of ethanol, and then mix and disperse by ultrasonication for 30 min. Add 1 mL of deionized water dropwise to the above mixture and ultrasonicate for 3 h to obtain nano-silica particles modified by HTPS and APTES.

[0085] 4) The modified nano-SiO2 particles and ethyl acetate are mixed, magnetically stirred and ultrasonically vibrated, and then a fluorosilicone resin-epoxy resin composite is added in a ratio of 1:1 and stirred evenly to obtain a coating solution.

[0086] The vinyl silane-modified core-shell structure composite material LaB6@SiO2 prepared in Example 1 was taken as a scanning electron microscope experimental sample, and the vinyl silane-modified core-shell structure composite materials obtained in Examples 1-5 and Comparative Examples 1-5 were taken as water contact angle experimental samples.

[0087] Figure 1 Transmission electron microscopy image of LaB6@SiO2 core-shell composite material modified with vinyl silane. Figure 1 It can be seen that the composite material obtained by the present invention is a core-shell structure.

[0088] Figure 2 This is the water contact angle diagram of the LaB6@SiO2 coating of the core-shell structure composite material modified by vinyl silane prepared in Example 1. Figure 3 The water contact angle diagram of the silicon dioxide coating prepared in Comparative Example 5 is shown in FIG. Figure 2 It can be seen that the water contact angle of the core-shell structure composite material LaB6@SiO2 modified by vinyl silane is 96.88°, and the water contact angle of silicon dioxide is 44.563°. It can be seen that the core-shell structure composite material LaB6@SiO2 modified by vinyl silane of the present invention has strong hydrophobicity. The water contact angles of the core-shell structure composite materials modified by vinyl silane obtained in Examples 1-5 and Comparative Examples 1-5 are statistically analyzed, and the results are shown in the following table:

[0089]

[0090] In addition, the core-shell structure composite material modified by vinyl silane obtained in Examples 1-5 and Comparative Examples 1-5 was subjected to an ice melting test. The coating samples of Examples 1-5 and Comparative Examples 1-5 were placed on the same height platform in a -20°C freezer, and sprayed with water mist using a spray gun. When the ice amount of each sample reached 30g, it was taken out and transferred to another dry -20°C freezer. After freezing for 24 hours, the ice melting test was started. During the ice melting test, ten samples were placed under the same power light source for irradiation at the same time, and the remaining ice amount of the samples was recorded. The analysis results are as follows: Figure 4 The figure shows the ice melting rate of Examples 1-5. It can be seen that since the amount of rare earth boride added in Examples 1-5 is almost constant, there is no obvious difference in the ice melting effect. Based on this phenomenon, we selected Example 1 and Comparative Examples 1-5 to draw the ice melting rate curve, as shown in FIG. Figure 5It can be seen that the ice melting rate curves of Comparative Examples 3 and 4 show subtle differences compared to the too little and too much rare earth addition in Example 1, that is, the complete ice melting time in Example 1, Comparative Examples 3 and 4 is 10min, 11min and 9min respectively, but the anti-icing effect shown by the contact angle data is significantly different. In Comparative Example 1, other rare earth borides not in the present invention are used for ice melting experiments. It can be seen that it also has a good ice melting effect but is not as good as the rare earth borides described in the present invention, and the cost is high, and it does not have the potential for wide application. The ice melting rate of Comparative Example 2 is greatly reduced. When the sample of Example 1 achieves complete ice melting, its ice amount is still 20g. This is because although the rare earth oxide has an absorption effect in a small range of bands, it does not have a good absorption capacity in the infrared band where ice mainly melts, so the ice melting effect is greatly reduced. For the coating without adding heat absorbing material in Comparative Example 5, it only has an effect on anti-icing, but no ice melting effect, so the ice melting rate in the curve is the worst, and 7g of ice is melted by light source irradiation only in 10min.

[0091] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A vinyl silane-modified core-shell composite material, characterized in that: The composite material is prepared from the following raw materials in parts by weight: Rare earth hexaboride 0.23-0.57 parts; 26.30-31.20 parts of basic catalyst; Silicon source 0.27-0.33 parts; Ethanol 66.36-72.56 parts; 0.60-0.89 parts of vinyl silane modifier; The rare earth hexaboride is one or more of LaB6, SmB6, and CeB6; The alkaline catalyst is one or more of sodium hydroxide, ammonia water and triethylamine; The silicon source is one or more of tetraethyl orthosilicate, methyltrimethoxysilane, and ammonium hexafluorosilicate; The vinyl silane modifier is one or more of vinyl triethoxysilane, vinyl triisopropoxysilane and vinyl tributylidene oxime silane.

2. The method for preparing the vinylsilane-modified core-shell structure composite material according to claim 1, characterized in that: The preparation method comprises the following steps: 1) Mixing rare earth hexaboride and ethanol and ultrasonically dispersing for 1-3 hours to obtain a mixed solution; 2) Add alkaline catalyst and silicon source to the mixed solution, stir at room temperature for 2-3 hours, and then centrifuge and wash to obtain core-shell structure ReB6@SiO2; 3) The core-shell structure ReB6@SiO2 is dispersed in ethanol, an alkaline catalyst is added to adjust to neutrality, and then a vinyl silane modifier is added. After stirring at 55-65°C for 18-24h, the vinyl silane-modified core-shell structure ReB6@SiO2 is obtained by filtering, washing and drying.

3. Use of the core-shell structure composite material modified by vinyl silane according to claim 1 in the preparation of an anti-icing and de-icing agent.

4. Use of the vinylsilane-modified core-shell structure composite material according to claim 1 in the preparation of railway deicing products.

Citation Information

Patent Citations

  • Method for preparing super-hydrophobic nano-magnetic thin film

    CN102336972A

  • Super thermal-insulation heat-preservation coating containing nanometer LaB6 powder and preparation method of coating