A heat treatment process and equipment for correcting deformation of steam turbine castings

Through the heat treatment process of segmented heating and gradient cooling, combined with a multi-angle correction mechanism and vibration aging, the problems of deformation and residual stress of steam turbine castings are solved, and precise correction and performance improvement of the castings are achieved.

CN118480651BActive Publication Date: 2024-10-18HANGZHOU STEAM TURBINE CASTING & FORGING
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410948664.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-10-18
Estimated Expiration
2044-07-16

AI Technical Summary

Technical Problem

Due to its irregular shape and material properties of high strength, high hardness, and high toughness, steam turbine castings are difficult to effectively correct deformation with existing heat treatment processes, and traditional methods are prone to generate new residual stress during the heating and cooling process, making the deformation problem difficult to solve.

Method used

It adopts the heat treatment process of segmented heating correction, gradient cooling and stress control, including cleaning and annealing in the pretreatment stage, the use of multi-angle correction mechanisms in the segmented heating stage, insulation optimization and gradient cooling, combined with vibration aging and shot peening. Ensure the uniformity and stability of the casting during the heating and cooling process.

Benefits of technology

It effectively reduces the deformation of the casting during the heating and cooling process, improves the shape accuracy and mechanical properties of the casting, enhances the strength, hardness and wear resistance of the casting, and ensures the correction effect and material stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118480651B_ABST
    Figure CN118480651B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of heat treatment of castings, and discloses a heat treatment process and equipment for correcting deformation of steam turbine castings, comprising the following steps: S1, pretreatment stage: cleaning and removing impurities from the castings; and performing stress relief annealing on the cleaned castings through an annealing furnace; S2, segmented heating correction: after annealing, castings with deformation are screened out, the castings are divided into a plurality of regions according to the deformation positions, the deformed regions are heated, and then the deformed regions are corrected in shape through a multi-angle correction mechanism; S4, gradient cooling and stress control: the castings are cooled in a gradient cold zone manner, the cooling time is 6-8 hours, and the castings are subjected to vibration aging during the cooling process, and the vibration aging time is 8 hours; the invention can effectively reduce the deformation of the castings during the heating and cooling processes through the steps of segmented heating correction, gradient cooling and stress control, so that the shape of the castings is more precise and meets the design requirements.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of heat treatment of castings, and more specifically to a heat treatment process and equipment for correcting deformation of steam turbine castings. Background Art

[0002] Castings are metal shaped objects obtained by various casting methods. Liquid metal is poured into a casting cavity that is adapted to the shape of the part, and after it cools and solidifies, a metal part with a certain shape, size and performance is obtained. Affected by factors such as the structure, material requirements, cooling conditions, casting process, and personnel operation of large machine tool castings, castings often produce a certain amount of deformation, especially castings with a long length (generally 6000-10000mm) and complex structure. The main factors of casting deformation are: residual stress, the internal stress generated during the casting process is released in the subsequent process, resulting in deformation; temperature change, the casting is deformed due to thermal expansion and contraction caused by uneven temperature during the cooling process or use; unreasonable structural design: the casting structure is not conducive to uniform force, and it is easy to deform, etc. The Chinese patent (CN116814914A) discloses "a heat treatment process for correcting the deformation of machine tool castings", which is suitable for the correction of large machine tool castings with large deformation caused by the casting process. The machine tool casting is placed on all pads with the concave surface facing downward and the convex surface facing upward, so that the maximum deformation of the machine tool casting is located at the pad in the center; a certain tonnage of pressure iron is placed on the deformed machine tool casting to make the casting elastically deformed, and then heated to 600-650°C at a heating rate of 30-50°C / h in a natural gas heat treatment furnace, and kept warm for a certain period of time, and slowly cooled to 150°C at a cooling rate of ≤30°C / h, and then cooled to room temperature with the furnace. This heat treatment process not only eliminates the residual stress of the casting, but also makes the deformed casting meet the processing and use requirements of the drawings, while not increasing the casting cost and reducing scrap losses, providing a stable heat treatment process for correcting the deformation problems generated during the production process of machine tool castings.

[0003] For irregular turbine castings such as turbine casing castings, it is difficult to achieve correction effects through existing processes. On the one hand, due to the irregular shape of the castings, it is difficult to correct them through conventional iron pressing due to directional restrictions. On the other hand, turbine castings are usually cast with high-strength, high-hardness and high-toughness materials, and it is difficult to achieve correction effects directly through iron pressing. Traditional heat treatment methods are prone to generate new residual stresses during heating and cooling, causing new deformations in the castings and failing to achieve good correction effects. Summary of the invention

[0004] In order to overcome the above-mentioned defects of the prior art, the present invention provides a heat treatment process and equipment for correcting the deformation of turbine castings, so as to solve the problem that it is difficult to achieve the correction effect for the characteristics of automobile wheel castings in the above-mentioned background technology; new residual stresses are easily generated during heat treatment, causing new deformation problems.

[0005] The present invention provides the following technical solution: A heat treatment process for correcting the deformation of a steam turbine casting, comprising the following steps:

[0006] S1, pre-processing stage:

[0007] Clean the castings to remove impurities;

[0008] The cleaned casting is subjected to stress relief annealing in an annealing furnace;

[0009] S2. Segmented heating correction: After annealing, cast pieces with deformation are screened out, and the cast pieces are divided into multiple areas according to the deformation positions. The deformed areas are heated, and then the shape of the deformed areas is corrected through a multi-angle correction mechanism;

[0010] S3, insulation optimization stage: after annealing, the castings without deformation and the castings after deformation correction are subjected to insulation treatment, the insulation temperature is 500℃, and the time is 2h-4h;

[0011] S4, gradient cooling and stress control: The casting is cooled by gradient cooling zone, the cooling time is 6-8h, and the casting is subjected to vibration aging during the cooling process, the vibration aging time is 8h;

[0012] S5. Post-processing strengthening: Shot peening treatment is performed to improve the quality and stability of the casting, and surface grinding, polishing and coating are performed.

[0013] Furthermore, the casting cleaning process in S1 comprises the following steps:

[0014] Step 1: Soak the casting in a soaking tank and add cleaning liquid into the soaking tank;

[0015] Step 2: Use a high-pressure spray gun to rinse the surface and interior of the casting in the immersion tank;

[0016] Step 3: After rinsing, the casting is cleaned by ultrasonic cleaning equipment.

[0017] Furthermore, the heating of the deformation area in S2 is divided into two stages:

[0018] The first stage: the deformation area of ​​the casting is heated from room temperature to 200℃-400℃ by resistance heating, and the heating rate is 30℃-50℃ / 1h;

[0019] The second stage: the deformation area of ​​the casting is heated from 200℃-400℃ to 750℃-900℃ by flame heating.

[0020] A heat treatment device for correcting the deformation of a steam turbine casting, comprising an annealing furnace and a multi-angle correction mechanism in a heat treatment process for correcting the deformation of a steam turbine casting, wherein the annealing furnace comprises a furnace wall, a plurality of electric heating devices are installed on both sides of the inner wall of the furnace wall, a vibration base is fixedly installed at the bottom of the furnace wall, a frame-shaped base is fixedly connected to the bottom of the vibration base, an air circulation mechanism is arranged inside the furnace wall, and a gate is installed at the front of the furnace wall;

[0021] The multi-angle correction mechanism includes a workbench, and the front and back sides of the workbench are fixedly connected with lateral movement components, and the output ends of the two lateral movement components are fixedly installed with semicircular rail arms. The side walls of the semicircular rail arms are provided with sliding mechanisms, and a rotating output mechanism is provided on one side of the sliding mechanism. The output end of the rotating output mechanism is installed with a hydraulic rod.

[0022] Furthermore, the air circulation mechanism includes two air inlet ducts, an air outlet cabin, several motors 1 and several motors 2. The two air inlet ducts are installed on the top of the inner wall of the furnace wall, and the air outlet cabin is installed inside the inner wall of the furnace wall. Several air inlet fans are arranged at the bottom of the two air inlet ducts, and several exhaust fans are arranged at the front of the air outlet cabin. Several motors 1 are fixedly installed on the top of the furnace wall, and their output shafts pass through the furnace wall and the air inlet duct and are respectively connected to the rotating shafts of several air inlet fans. Several motors 2 are fixedly installed on the back of the furnace wall, and their output shafts pass through the furnace wall and the air outlet cabin and are respectively connected to the rotating shafts of several exhaust fans. The interiors of the two air inlet ducts are connected with the interiors of the air outlet cabins through two connecting ducts.

[0023] Furthermore, the vibration base includes a main base body, a recess is provided on the top of the main base body, a vibration base body is movably connected in the recess, a through hole is provided at the bottom of the main base body and the through hole is provided with an exciter, and the exciter is fixedly installed at the bottom of the vibration base body.

[0024] Furthermore, the longitudinal cross-section of the vibration seat body is T-shaped, and the longitudinal cross-section of the notch on the top of the main seat body is T-shaped.

[0025] Furthermore, an electric heating pipe is fixedly installed inside the air inlet cabin.

[0026] Furthermore, the sliding mechanism includes a sliding sleeve, which is slidably connected to the side wall of the semicircular rail arm, a motor three is fixedly installed on the top of the sliding sleeve, a gear one is fixedly installed on the output shaft of the motor three, a tooth groove is opened on the side wall of the semicircular rail arm, and one side wall of the gear is meshed in the tooth groove of the side wall of the semicircular rail arm, and the rotary output mechanism is arranged on one side of the sliding sleeve.

[0027] Furthermore, the rotary output mechanism includes a rotary column and a motor four. A rotary hole is opened on one side of the sliding sleeve, and the rotary column is movably sleeved in the rotary hole. The motor four is fixedly installed at the bottom of the sliding sleeve. The side wall of the rotary column is fixedly connected to a gear ring. The output shaft of the motor four is fixedly connected to a gear two, and the gear two is meshed with the gear ring. A connecting plate is fixedly connected to one side of the rotary column, and the connecting plate is the output end of the rotary output mechanism.

[0028] Technical effects and advantages of the present invention:

[0029] The present invention can effectively reduce the deformation of the casting during the heating and cooling process through the steps of segmented heating correction, gradient cooling and stress control, so that the shape of the casting is more precise and meets the design requirements. After the steps of fine pretreatment, thermal insulation optimization and post-treatment strengthening, the residual stress inside the casting is eliminated and the structure of the material is optimized, thereby improving the mechanical properties of the casting such as strength, hardness and wear resistance, and enhancing the quality and stability of the casting.

[0030] Before stress annealing of castings, a cleaning process is added to remove excess impurities on the surface of castings. On the one hand, impurities on the surface of castings, such as oil, rust, oxides, etc., are prevented from hindering heat transfer during annealing and affecting the annealing effect. On the other hand, impurities on the surface of castings are prevented from generating stress due to uneven heating during annealing, which may cause deformation of castings. Before casting correction, a segmented heating process is added to change the mechanical properties of the material, enhance the plasticity of the correction area, facilitate subsequent correction operations, and reduce the risk of cracks or damage during the correction process.

[0031] During the annealing stage of the casting in the annealing furnace, improvements are made to the traditional annealing furnace. In the heating stage, the wind circulation mechanism is used to circulate hot air so that the entire casting can be evenly heated to avoid the generation of new internal stress during the annealing heating stage of the casting. In the cooling stage, the wind circulation mechanism and the vibration base are used to cooperate. On the one hand, the casting can be cooled evenly and the cooling speed can be controlled to avoid the generation of new internal stress. On the other hand, residual internal stress can be eliminated.

[0032] When the casting is corrected by the multi-angle correction mechanism, the sliding mechanism and the rotating output mechanism can be used to change the correction position and direction according to the shape of the casting, so that the device can adapt to the irregular castings of the steam turbine to achieve precise correction effects and is more flexible. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a schematic diagram of the overall structure of the annealing furnace of the present invention;

[0034] Figure 2 For the present invention Figure 1 Explosion diagram of the wind circulation mechanism structure;

[0035] Figure 3 It is an exploded schematic diagram of the overall structure of the annealing furnace of the present invention;

[0036] Figure 4 For the present invention Figure 3 A schematic diagram of the longitudinal section structure of the main seat body and the vibration seat body;

[0037] Figure 5 For the present invention Figure 2 Schematic diagram of the cross-sectional structure of the air inlet duct;

[0038] Figure 6 It is a schematic diagram of the overall structure of the multi-angle correction mechanism of the present invention;

[0039] Figure 7 For the present invention Figure 6 Schematic diagram of the sliding mechanism and rotating output mechanism structure.

[0040] The accompanying drawings are marked as follows: 1. furnace wall; 2. electric heating device; 3. vibration base; 4. frame base; 5. air circulation mechanism; 51. air inlet cabin; 52. air outlet cabin; 53. air inlet fan; 54. exhaust fan; 55. motor one; 56. motor two; 57. connecting cabin; 58. electric heating pipe; 31. main seat body; 32. vibration seat body; 33. exciter; 6. workbench; 7. lateral movement assembly; 8. semicircular rail arm; 9. sliding mechanism; 10. rotary output mechanism; 11. hydraulic rod; 91. sliding sleeve; 92. motor three; 93. gear one; 101. rotary column; 102. motor four; 103. gear two; 104. gear ring; 105. connecting plate. DETAILED DESCRIPTION

[0041] The specific implementation modes of the present invention are described in detail below with reference to the accompanying drawings.

[0042] Embodiment 1

[0043] The present invention provides a heat treatment process for correcting deformation of a steam turbine casting, comprising the following steps:

[0044] S1, pre-processing stage:

[0045] Clean the castings to remove impurities to avoid uneven heating and cooling caused by impurities;

[0046] The cleaned castings are subjected to stress relief annealing in an annealing furnace to eliminate the residual stress generated during the casting process and prevent deformation;

[0047] S2. Segmented heating correction: After annealing, cast pieces with deformation are screened out, and the cast pieces are divided into multiple areas according to the deformation positions. The deformed areas are heated, and then the shape of the deformed areas is corrected through a multi-angle correction mechanism;

[0048] S3, insulation optimization stage: after annealing, the castings without deformation and the castings after deformation correction are subjected to insulation treatment at a temperature of 500°C for 2 hours to improve the internal structure of the castings;

[0049] S4, gradient cooling and stress control: The casting is cooled by gradient cooling zone, and the cooling speed is gradually reduced from high temperature to low temperature. The cooling time is 6 hours. During the cooling process, the casting is subjected to vibration aging, and the vibration aging time is 8 hours to prevent new deformation and stress.

[0050] S5. Post-processing strengthening: Shot peening treatment is performed to improve the quality and stability of the castings, and surface grinding, polishing and coating are performed to improve the aesthetics.

[0051] Preferably, the casting cleaning process in S1 comprises the following steps:

[0052] Step 1: Soak the casting in a soaking tank and add cleaning liquid into the soaking tank;

[0053] Step 2: Use a high-pressure spray gun to rinse the surface and interior of the casting in the immersion tank to remove oil stains and larger attached impurities;

[0054] Step 3: After rinsing, the casting is cleaned by ultrasonic cleaning equipment to remove smaller impurities attached to the surface of the casting and difficult-to-remove oil stains.

[0055] Reference Figure 2 , the heating of the deformation area in S2 is divided into two stages:

[0056] The first stage: the deformation area of ​​the casting is heated from room temperature to 200°C by resistance heating, with a heating rate of 30°C / 1h. Preheating by slow heating can reduce stress generation;

[0057] The second stage: The deformation area of ​​the casting is heated from 200°C to 750°C by flame heating. After heating, the local plasticity of the casting is increased, making it easier to deform and making the external force correction process easier.

[0058] Reference Figure 1 , 6A heat treatment device for correcting the deformation of a steam turbine casting, comprising an annealing furnace and a multi-angle correction mechanism in a heat treatment process for correcting the deformation of a steam turbine casting, characterized in that: the annealing furnace comprises a furnace wall 1, a plurality of electric heating devices 2 are installed on both sides of the inner wall of the furnace wall 1, a vibration base 3 is fixedly installed at the bottom of the furnace wall 1, a frame-shaped base 4 is fixedly connected to the bottom of the vibration base 3, an air circulation mechanism 5 is arranged inside the furnace wall 1, and a gate is installed on the front of the furnace wall 1; when in use, the casting is placed on the inner wall of the furnace wall 1 and fixed on the top of the vibration base 3, and the gate is closed after the casting The casting enters the heating stage and is heated by the vibrating base 3. During this process, the wind circulation mechanism 5 is operated to circulate hot air inside the furnace wall 1, promoting uniform temperature distribution inside the furnace wall 1, facilitating uniform heating of the casting, thereby avoiding new internal stress caused by uneven heating of the casting during heating. During the cooling stage, the gate is opened to allow auxiliary air cooling to be run through the wind circulation mechanism 5 to slowly cool the casting, and at the same time facilitate uniform cooling of the casting. During this process, the vibrating base 3 is operated to vibrate the casting, which can further eliminate residual internal stress of the casting.

[0059] The multi-angle correction mechanism includes a workbench 6, and the front and back sides of the workbench 6 are fixedly connected to lateral movement components 7. Semicircular rail arms 8 are fixedly installed on the output ends of the two lateral movement components 7. The side walls of the semicircular rail arms 8 are provided with sliding mechanisms 9. A rotary output mechanism 10 is provided on one side of the sliding mechanism 9. A hydraulic rod 11 is installed on the output end of the rotary output mechanism 10. The steam turbine casting is placed on the top of the workbench 6, and then the semicircular rail arms 8 are driven to move horizontally through the output of the lateral movement component 7, so that the hydraulic rod 11 moves to the deformation area of ​​the casting, and then the sliding mechanism 9 is operated to slide along the side walls of the semicircular rail arms 8. According to the shape characteristics of the semicircular rail arms 8, the hydraulic rod 11 is made to surround the casting, thereby adjusting the position and output direction of the hydraulic rod 11, and the rotary output mechanism 10 output drives the hydraulic rod 11 to rotate, so that the output direction of the hydraulic rod 11 can be further adjusted, thereby adapting to irregular-shaped steam turbine castings.

[0060] Reference Figure 2The air circulation mechanism 5 includes two air inlet cabins 51, an air outlet cabin 52, a plurality of motors 1 55, and a plurality of motors 2 56. The two air inlet cabins 51 are installed on the top of the inner wall of the furnace wall 1, and the air outlet cabin 52 is installed inside the inner wall of the furnace wall 1. A plurality of air inlet fans 53 are arranged at the bottom of the two air inlet cabins 51, and a plurality of exhaust fans 54 are arranged on the front of the air outlet cabin 52. The plurality of motors 1 55 are fixedly installed on the top of the furnace wall 1, and the output shafts of the plurality of motors 1 55 penetrate the furnace wall 1 and the air inlet cabins 51 are respectively connected to the rotating shafts of the plurality of air inlet fans 53. The plurality of motors 2 56 are fixedly installed on the back of the furnace wall 1, and the output shafts of the plurality of motors 2 56 penetrate the furnace wall 1. The wall 1 and the air outlet chamber 52 are respectively connected to the rotating shafts of several exhaust fans 54. The interiors of the two air inlet cabins 51 are connected with the interior of the air outlet cabin 52 through two connecting cabins 57. When working, the motor 1 55 outputs power to drive the air inlet fan 53 to operate, so that the upper air inside the furnace wall 1 is input into the air inlet cabin 51, and the airflow enters the air outlet cabin 52. The motor 2 56 outputs power to drive the exhaust fan 54 to operate, so that the air is output to the inside of the furnace wall 1 again. The airflow direction flows from the back of the furnace wall 1 to the front direction, thereby achieving an internal circulation effect, avoiding uniform temperature distribution inside the furnace wall 1, and uniformly heating the casting.

[0061] Reference Figure 3 The vibration base 3 includes a main base body 31, a notch is provided on the top of the main base body 31, and a vibration base body 32 is movably connected in the notch. A through hole connected to the notch is provided at the bottom of the main base body 31, and an exciter 33 is provided at the through hole. The exciter 33 is fixedly installed at the bottom of the vibration base body 32, and the casting needs to be fixed on the top of the vibration base body 32. When the vibration base 3 is working, the vibration base body 32 is driven to vibrate by the operation of the exciter 33. Since the casting is fixed on the top of the vibration base 3, the casting can achieve the excitation effect.

[0062] Reference Figure 4 The longitudinal section of the vibration seat body 32 is T-shaped, and the longitudinal section of the top notch of the main seat body 31 is T-shaped. This arrangement can prevent the vibration seat body 32 from falling off from the top notch of the main seat body 31.

[0063] Reference Figure 5 An electric heating pipe 58 is fixedly installed inside the air inlet chamber 51. By setting the electric heating pipe 58, the temperature of the airflow output by the air circulation mechanism 5 to the inside of the furnace wall 1 can be controlled. When the casting annealing enters the cooling stage, the temperature control effect of the airflow output by the air circulation mechanism 5 can facilitate the control of the cooling speed of the casting, thereby avoiding new internal stress and deformation.

[0064] Reference Figure 7The sliding mechanism 9 includes a sleeve 91, which is slidably sleeved on the side wall of the semicircular rail arm 8. A motor 3 92 is fixedly installed on the top of the sleeve 91, and a gear 1 93 is fixedly installed on the output shaft of the motor 3 92. A tooth groove is opened on the side wall of the semicircular rail arm 8, and the side wall of the gear 1 93 meshes in the tooth groove of the side wall of the semicircular rail arm 8. The rotary output mechanism 10 is arranged on one side of the sleeve 91. When the motor 3 92 outputs, it drives the gear 1 93 to rotate. Through the meshing relationship between the gear 1 93 and the tooth groove of the side wall of the semicircular rail arm 8, the sleeve 91 slides on the side wall of the semicircular rail arm 8, thereby making the sliding mechanism 9 slide on the side wall of the semicircular rail arm 8.

[0065] Reference Figure 7 The rotary output mechanism 10 includes a rotary column 101 and a motor 4 102. A rotary hole is provided on one side of the sleeve 91. The rotary column 101 is movably sleeved in the rotary hole. The motor 4 102 is fixedly installed at the bottom of the sleeve 91. A gear ring 104 is fixedly connected to the side wall of the rotary column 101. The output shaft of the motor 4 102 is fixedly connected to a gear 2 103. The gear 2 103 is meshed with the gear ring 104. A connecting plate 105 is fixedly connected to one side of the rotary column 101. The connecting plate 105 is the output end of the rotary output mechanism 10. When working, the motor 4 102 outputs power to drive the gear 2 103 to rotate. Through the meshing relationship between the gear 2 103 and the gear ring 104, the rotary column 101 drives the connecting plate 105 to rotate, thereby causing the hydraulic rod 11 to rotate and rotate.

[0066] Embodiment 2

[0067] The present invention provides a heat treatment process for correcting deformation of a steam turbine casting, comprising the following steps:

[0068] S1, pre-processing stage:

[0069] Clean the castings to remove impurities;

[0070] The cleaned casting is subjected to stress relief annealing in an annealing furnace;

[0071] S2. Segmented heating correction: After annealing, cast pieces with deformation are screened out, and the cast pieces are divided into multiple areas according to the deformation positions. The deformed areas are heated, and then the shape of the deformed areas is corrected through a multi-angle correction mechanism;

[0072] S3, insulation optimization stage: after annealing, castings without deformation and castings after deformation correction are subjected to insulation treatment at a temperature of 500°C for 4 hours;

[0073] S4, gradient cooling and stress control: The casting is cooled by gradient cooling zone, the cooling time is 8 hours, and the casting is subjected to vibration aging during the cooling process, the vibration aging time is 8 hours;

[0074] S5. Post-processing strengthening: Shot peening treatment is performed to improve the quality and stability of the castings, and surface grinding, polishing and coating are performed to improve the aesthetics.

[0075] Preferably, the casting cleaning process in S1 comprises the following steps:

[0076] Step 1: Soak the casting in a soaking tank and add cleaning liquid into the soaking tank;

[0077] Step 2: Use a high-pressure spray gun to rinse the surface and interior of the casting in the immersion tank;

[0078] Step 3: After rinsing, the casting is cleaned by ultrasonic cleaning equipment.

[0079] Reference Figure 2 , the heating of the deformation area in S2 is divided into two stages:

[0080] The first stage: the deformation area of ​​the casting is heated from room temperature to 300°C by resistance heating, with a heating rate of 50°C / 1h;

[0081] The second stage: the deformation area of ​​the casting is heated from 300°C to 800°C by flame heating.

[0082] Embodiment 3

[0083] The present invention provides a heat treatment process for correcting deformation of a steam turbine casting, comprising the following steps:

[0084] S1, pre-processing stage:

[0085] Clean the castings to remove impurities;

[0086] The cleaned casting is subjected to stress relief annealing in an annealing furnace;

[0087] S2. Segmented heating correction: After annealing, cast pieces with deformation are screened out, and the cast pieces are divided into multiple areas according to the deformation positions. The deformed areas are heated, and then the shape of the deformed areas is corrected through a multi-angle correction mechanism;

[0088] S3, insulation optimization stage: after annealing, castings without deformation and castings after deformation correction are subjected to insulation treatment at a temperature of 500°C for 4 hours;

[0089] S4, gradient cooling and stress control: The casting is cooled by gradient cooling zone, the cooling time is 8 hours, and the casting is subjected to vibration aging during the cooling process, the vibration aging time is 8 hours;

[0090] S5. Post-processing strengthening: Shot peening treatment is performed to improve the quality and stability of the castings, and surface grinding, polishing and coating are performed to improve the aesthetics.

[0091] Preferably, the casting cleaning process in S1 comprises the following steps:

[0092] Step 1: Soak the casting in a soaking tank and add cleaning liquid into the soaking tank;

[0093] Step 2: Use a high-pressure spray gun to rinse the surface and interior of the casting in the immersion tank;

[0094] Step 3: After rinsing, the casting is cleaned by ultrasonic cleaning equipment.

[0095] Reference Figure 2 , the heating of the deformation area in S2 is divided into two stages:

[0096] The first stage: the deformation area of ​​the casting is heated from room temperature to 400°C by resistance heating, with a heating rate of 50°C / 1h;

[0097] The second stage: the deformation area of ​​the casting is heated from 400°C to 900°C by flame heating.

[0098] The following table shows the selection of segmented heating correction parameters and the comparison with no heating

[0099] First stage temperature Heating rate Second stage temperature Number of experiments Number of damaged casting surfaces The amount of new variable stress generated in the casting Embodiment 1 200℃ 30℃ / 1h 750℃ 20 0 0 Embodiment 2 300℃ 50℃ / 1h 800℃ 20 0 1 Implementation Column 3 400℃ 50℃ / 1h 900℃ 20 2 3 No stage heating 20 8 0

[0100] The above shows and describes the basic principles, main features and advantages of the present invention. The present invention is not limited to the above embodiments. The above embodiments and descriptions are only for explaining the principles of the present invention. The present invention may be subject to various changes and improvements without departing from the spirit and scope of the present invention. These changes and improvements fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A heat treatment process for correcting deformation of steam turbine castings, characterized in that: The following steps are involved: S1, pre-processing stage: Clean the castings to remove impurities; The cleaned casting is subjected to stress relief annealing in an annealing furnace; The annealing furnace comprises a furnace wall (1), a plurality of electric heating devices (2) are installed on both sides of the inner wall of the furnace wall (1), a vibration base (3) is fixedly installed at the bottom of the furnace wall (1), and a frame-shaped base (4) is fixedly connected to the bottom of the vibration base (3), and the vibration base (3) comprises a main base body (31), a notch is provided at the top of the main base body (31), and a vibration base body (32) is movably connected in the notch, and a through hole is provided at the bottom of the main base body (31) and communicates with the notch, and an exciter (33) is arranged at the through hole, and the exciter (33) is fixedly installed at the bottom of the vibration base body (32), the longitudinal cross section of the vibration base body (32) is T-shaped, and the longitudinal cross section of the notch at the top of the main base body (31) is T-shaped; During the cooling stage, the casting is vibrated by the operation of the vibrating base (3) to further eliminate the residual internal stress of the casting; S2. Segmented heating correction: After annealing, cast pieces with deformation are screened out, and the cast pieces are divided into multiple areas according to the deformation positions. The deformed areas are heated, and then the shape of the deformed areas is corrected through a multi-angle correction mechanism. The multi-angle correction mechanism comprises a workbench (6), the front and back sides of the workbench (6) are fixedly connected to lateral movement components (7), the output ends of the two lateral movement components (7) are fixedly mounted with semicircular rail arms (8), the side walls of the semicircular rail arms (8) are provided with sliding mechanisms (9), one side of the sliding mechanism (9) is provided with a rotary output mechanism (10), and the output end of the rotary output mechanism (10) is mounted with a hydraulic rod (11); S3, insulation optimization stage: after annealing, the castings without deformation and the castings after deformation correction are subjected to insulation treatment, the insulation temperature is 500℃, and the time is 2h-4h; S4, gradient cooling and stress control: The casting is cooled by gradient cooling zone, the cooling time is 6-8h, and the casting is subjected to vibration aging during the cooling process, the vibration aging time is 8h; S5. Post-processing strengthening: Shot peening treatment is performed to improve the quality and stability of the casting, and surface grinding, polishing and coating are performed.

2. A heat treatment process for correcting deformation of steam turbine castings according to claim 1, characterized in that: The casting cleaning process in S1 has the following steps: Step 1: Soak the casting in a soaking tank and add cleaning liquid into the soaking tank; Step 2: Use a high-pressure spray gun to rinse the surface and interior of the casting in the immersion tank; Step 3: After rinsing, the casting is cleaned by ultrasonic cleaning equipment.

3. A heat treatment process for correcting deformation of steam turbine castings according to claim 1, characterized in that: The heating of the deformation area in S2 is divided into two stages: The first stage: the deformation area of ​​the casting is heated from room temperature to 200℃-400℃ by resistance heating, and the heating rate is 30℃-50℃ / 1h; The second stage: the deformation area of ​​the casting is heated from 200℃-400℃ to 750℃-900℃ by flame heating.

4. A heat treatment device for correcting the deformation of a steam turbine casting, comprising an annealing furnace and a multi-angle correction mechanism in a heat treatment process for correcting the deformation of a steam turbine casting according to claim 1, characterized in that: An air circulation mechanism (5) is arranged inside the furnace wall (1), a gate is arranged on the front of the furnace wall (1), and the air circulation mechanism (5) comprises two air inlet ducts (51), an air outlet chamber (52), a plurality of motors 1 (55), and a plurality of motors 2 (56). The two air inlet ducts (51) are arranged on the top of the inner wall of the furnace wall (1), the air outlet chamber (52) is arranged inside the inner wall of the furnace wall (1), a plurality of air inlet fans (53) are arranged at the bottom of the two air inlet ducts (51), and a plurality of exhaust fans (53) are arranged on the front of the air outlet chamber (52). 54), a plurality of motors 1 (55) are fixedly installed on the top of the furnace wall (1), and the output shafts of the plurality of motors 1 (55) penetrate the furnace wall (1) and the air inlet chamber (51) and are respectively connected to the rotating shafts of the plurality of air inlet fans (53); a plurality of motors 2 (56) are fixedly installed on the back of the furnace wall (1), and the output shafts of the plurality of motors 2 (56) penetrate the furnace wall (1) and the air outlet chamber (52) and are respectively connected to the rotating shafts of the plurality of air exhaust fans (54); the interiors of the two air inlet chambers (51) are respectively connected to the interiors of the air outlet chambers (52) via two connecting chambers (57).

5. The heat treatment equipment for correcting deformation of steam turbine castings according to claim 4, characterized in that: An electric heating pipe (58) is fixedly installed inside the air inlet chamber (51).

6. The heat treatment equipment for correcting deformation of steam turbine castings according to claim 4, characterized in that: The sliding mechanism (9) comprises a sliding sleeve (91), the sliding sleeve (91) is slidably sleeved on the side wall of the semicircular rail arm (8), a motor three (92) is fixedly mounted on the top of the sliding sleeve (91), a gear one (93) is fixedly mounted on the output shaft of the motor three (92), a tooth groove is formed on the side wall of the semicircular rail arm (8), and the side wall of the gear one (93) meshes in the tooth groove of the side wall of the semicircular rail arm (8), and the rotary output mechanism (10) is arranged on one side of the sliding sleeve (91).

7. The heat treatment equipment for correcting deformation of steam turbine castings according to claim 6, characterized in that: The rotary output mechanism (10) comprises a rotary column (101) and a motor four (102). A rotary hole is provided on one side of the sliding sleeve (91). The rotary column (101) is movably sleeved in the rotary hole. The motor four (102) is fixedly installed at the bottom of the sliding sleeve (91). A gear ring (104) is fixedly connected to the side wall of the rotary column (101). The output shaft of the motor four (102) is fixedly connected to a gear two (103). The gear two (103) meshes with the gear ring (104). A connecting plate (105) is fixedly connected to one side of the rotary column (101). The connecting plate (105) is the output end of the rotary output mechanism (10).

Citation Information

Patent Citations

  • Heat treatment process for correcting deformation of machine tool casting

    CN116814914A

  • Energy-saving annealing furnace

    CN104294016A

  • Rotary driving mechanism and bidirectional correction device for incomplete arc workpiece

    CN106825127A

  • Iron element control method for martensitic stainless steel 2Cr13 blade

    CN113084087A

  • Circular furnace inner cover roundness correcting machine

    CN114951466A