A method for detecting the element composition content of blast furnace wall condensed slag and its application

Through a combination of carbon and sulfur analysis, infrared carbon and sulfur analysis and glass melting-X-ray fluorescence spectrometry, combined with carbon value calibration and ignition coefficient inversion, the complexity of the carbon base material in the detection of condensed slag on the blast furnace wall is solved. , achieving fast and accurate elemental composition analysis and data correction, improving detection efficiency and reliability.

CN118483369BActive Publication Date: 2024-10-18SHANDONG IRON & STEEL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410933416.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-18
Estimated Expiration
2044-07-12

AI Technical Summary

Technical Problem

The existing technology is difficult to effectively detect the composition of primary and secondary elements in blast furnace wall condensation slag containing carbon base materials, and the detection method is complex, which can easily lead to instrument damage and data deviation.

Method used

Using carbon and sulfur analysis or infrared carbon and sulfur analysis combined with gravity burning method and glass melting-X-ray fluorescence spectrometry, through the back calculation of carbon value calibration coefficient and burning coefficient, the detection process is optimized to avoid data inaccuracy and introduce Half-weight weighing concept to correct test results.

Benefits of technology

It achieves rapid and accurate detection of condensed slag on the blast furnace wall, reduces detection costs, improves detection efficiency, ensures the reliability of data through multiple method verifications, and provides a comprehensive diagnostic basis for blast furnace working conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention relates to the field of chemical analysis and detection, and specifically to a detection method for the elemental composition content of blast furnace wall condensed slag and its application. The detection method provided by the present invention can detect the composition and content of each major and minor element in blast furnace wall condensed slag with various complex mineral phase bases including carbon-based materials, and in actual applications, when a large number of samples are detected using the method of the present invention, the measured results can be compared with each other without easily generating deviations, thereby solving the problem that once the blast furnace wall inclusions are carbon-based materials in the actual detection of blast furnace wall condensed slag, the detection cannot be continued due to over-range and damage to the detection instrument, thereby improving the detection system of the entire blast furnace wall condensed slag, producing a data array to feed back production, and realizing the comprehensive diagnosis of blast furnace working conditions using the detection results of blast furnace wall condensed slag.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of chemical analysis and detection, in particular to a method for detecting the element composition content of blast furnace wall condensed slag and an application thereof. Background Art

[0002] The condensed slag of the blast furnace wall, or blast furnace wall slag, blast furnace wall inclusions, is a mineral phase corrosion layer gradually formed in the blast furnace hearth, furnace wall and furnace bottom after the charge and the original refractory material fully react and run-in at high temperature. Its base is formed by the materials in the furnace under high temperature over the years, and it is rich in 15 common metallurgical elements such as carbon, iron, silicon, calcium, aluminum, magnesium, sulfur, phosphorus, titanium, potassium, sodium, lead, zinc, arsenic, and copper brought from the charge. In-depth analysis of the distribution of major and minor elements in each mineral phase corrosion layer can understand the impact of changes in operating parameters on blast furnace erosion, provide data guidance for optimizing blast furnace structure design and blast furnace maintenance, and is of great significance in the technical maintenance of ironmaking, especially in the diagnosis and improvement of furnace conditions during blast furnace overhaul.

[0003] The condensed slag of the blast furnace wall is essentially a unique mixture, with the characteristics of coke residue and molten iron residue condensed together. It involves many elements and the content distribution is extremely unclear. At present, there is no clear inspection guidance method for this type of substance in the national standard. Due to the chemical reaction characteristics of the blast furnace from top to bottom, as well as the influence of the phase fluctuation of the incoming charge and the habit of changing the batching at any time, the chemical composition of the erosion condensate sampled at different positions in the furnace is also different, and generally has the characteristics of "one furnace, one indicator". This differentiation is reflected in the field of chemical analysis, which requires the laboratory to make reasonable plans based on the existing configuration conditions, organize and simplify the overall complex problems, and use the existing inspection methods to optimize the decomposition of the above-mentioned elements in batches, so as to achieve the purpose of successfully completing more accurate inspections in a relatively economical and fast way.

[0004] Gravity burning method, carbon and sulfur determination instrument method, infrared carbon and sulfur method and glass melting-X-ray fluorescence spectrometry are all routine inspection methods in metallurgical chemical laboratories. They are widely and reliably used in the full analysis of coal coke, carbon and sulfur analysis of carbon-based materials, carbon and sulfur analysis of non-carbon-based materials, and full component analysis of iron ore powder samples. The powder state of blast furnace wall condensed slag also happens to concentrate the basic characteristics of the above four material forms, which can create experimental conditions for the inspection of related wall slag materials. After the subject target is disassembled, the above four methods are used to jointly determine its components. However, the complexity of the mineral phase of blast furnace wall condensed slag itself and its different components at various locations in the blast furnace bring great obstacles to the indiscriminate combination of the four methods.

[0005] The Chinese non-patent literature "Accurate determination and removal of residual carbon in the detection of major and minor components in blast furnace wall inclusions by X-ray fluorescence spectrometry" (Qi Bing, Zhang Qingfeng, Ju Yanmei, et al. Accurate determination and removal of residual carbon in the detection of major and minor components in blast furnace wall inclusions by X-ray fluorescence spectrometry [J]. Physical and Chemical Testing - Chemical Volume, 2023, 59(08): 970-973.) discloses a method for detecting major and minor components in blast furnace wall inclusions. However, this method ignores the complex situation of blast furnace wall inclusion types in actual detection, and is only a single idea. In actual application, once the blast furnace wall inclusions are carbon-based, it will cause over-range and unable to continue detection, and damage the detection instrument. However, the situation of carbon-based inclusions in blast furnace wall inclusions is inevitable and cannot be ignored in actual detection. Summary of the invention

[0006] The technical problem to be solved by the present invention is to provide a method for detecting the elemental composition content of blast furnace wall condensed slag and its application. The detection method provided by the present invention can detect the composition and content of major and minor elements in blast furnace wall condensed slag with various complex mineral phase bases including carbon-based materials, and in actual applications, when a large number of samples are detected using the method of the present invention, the measured results can be compared with each other without easily causing deviations, thereby improving the detection system of the entire blast furnace wall condensed slag, producing a data array to feed back production, and realizing the comprehensive diagnosis of blast furnace operating conditions using the blast furnace wall condensed slag detection results.

[0007] In summary, the present invention is an economical and fast method that first pre-judges and classifies the sample's mineral carbon base, then pre-treats the sample with a carbon and sulfur determination instrument or an infrared carbon and sulfur instrument in combination with a gravity burning method, then detects the sample composition after burning by glass melting film-X-ray fluorescence spectrometry, and finally restores the composition content of each major and minor amount of the blast furnace wall condensed slag material by reverse calculation through the burning coefficient. The key technology is that the samples taken from different positions of the blast furnace wall condensed slag material have very different innate components, especially because of the difference in carbon elements caused by the addition of carbon-based materials such as coal coke into the mineral phase, which will play a key role in which instrument and method are used to complete the subsequent inspection, and it is necessary to perform certain carbon-based estimation and sample pre-treatment in the early stage. The present invention takes into account the correction of the same data source under different methods, and introduces an intermediate composite material with both mineral-based and carbon-based characteristics to perform multi-method cross-measurement and calculate coefficient calibration, so that all inspection data can be issued under the same validity conditions, which greatly avoids the problem of lateral data inaccuracy caused by too many methods and standards adopted in the process. Specifically, according to the requirements of blast furnace inspection, all elements to be inspected are classified into detectable types. For carbon elements that are not suitable for glass melting film-X fluorescence spectrometry, infrared carbon-sulfur method or carbon and sulfur determination instrument are used to determine their content, and the carbon content space is predicted. The carbon values ​​measured by different carbon measurement methods are firstly corrected by coefficient regression, and gravity burning method is used to remove carbon and calculate its burning coefficient at the same time. Sufficient molten sample residue samples are reserved. When the sample is insufficient, the concept of half-weighing is introduced to correct the fluorescence coefficient of the test results. Finally, the glass melting film process is introduced with reference to the iron ore detection method, and other element components are concentratedly detected using an X-ray fluorescence spectrometer with a pre-built full element curve. After collecting the results, the component results are multiplied by the previously converted burning coefficient to obtain other components except carbon. The carbon element results are combined to obtain the total major and minor element composition content of the batch of blast furnace wall condensed slag.

[0008] Compared with other complicated technologies, the present invention has the characteristics of low application starting point, easy to learn, etc. It borrows the common inspection equipment and parameter accessories of the laboratory, optimizes and integrates the common inspection and testing methods, so that it has the advantages of fast inspection time, many elements that can be inspected at one time, and low inspection cost, etc., which can meet the rigid requirements of batch inspection and expedited inspection of the blast furnace. At the same time, its process characteristics also determine that according to the requirements of the inspection party for the precision of the overall data, the complexity of the experiment can be appropriately adjusted, and appropriate simplification or omission can be made on individual non-main processes, so that the overall presentation is to replace individual fine data with batch rough data to quantitatively reflect the composition rules of each element at the sampling position of the condensed slag material of the blast furnace wall. Finally, a variety of data validity verification methods are also provided, that is, after all inspections are completed, the carbon values, sulfur values, and even iron values ​​determined by two or more different methods can be compared with each other, and whether the weighting of all components reaches or approaches 100% can be verified to verify the relative reliability of the experiment. The final arrangement of the results of the composition and content of each element can basically be regarded as an indifferent number array produced under the same rule standard, which has the function of horizontal reference and comparison of all elements. It provides a basis for the iron-making department to use the blast furnace wall solidified slag to study and diagnose the furnace condition and steadily extend the life of the blast furnace.

[0009] The present invention provides a method for detecting the element composition content of blast furnace wall condensed slag, comprising the following steps: A) performing carbon determination and sulfur determination analysis or infrared carbon-sulfur analysis on the blast furnace wall condensed slag to obtain the carbon content and sulfur content of the blast furnace wall condensed slag; the blast furnace wall condensed slag comprises a carbon-based material, an intermediate composite material and a mineral-based material, wherein the carbon-based material is subjected to carbon determination and sulfur determination analysis, the mineral-based material is subjected to infrared carbon-sulfur analysis, and the intermediate composite material can be subjected to any one of carbon determination and sulfur determination analysis or infrared carbon-sulfur analysis;

[0010] If a fixed carbon and fixed sulfur analysis is performed, the results obtained from the fixed carbon and fixed sulfur analysis need to be calibrated according to the carbon value calibration coefficient a and the sulfur value calibration coefficient a';

[0011] The carbon calibration coefficient a is the ratio of the carbon content in the analysis results obtained by performing a fixed carbon and fixed sulfur analysis and an infrared carbon and sulfur analysis on the intermediate composite material;

[0012] The sulfur calibration coefficient a' is the ratio of the sulfur content in the analysis results obtained by performing a fixed carbon and fixed sulfur analysis on the intermediate composite material and performing an infrared carbon and sulfur analysis;

[0013] B) burning the blast furnace wall condensed slag obtained in step A) until it is carbon-free according to the carbon content of the blast furnace wall condensed slag obtained in step A), and collecting all carbon-free residues;

[0014] C) subjecting the carbon-free residue obtained in step B) to glass melting film-X-ray fluorescence spectrum detection to obtain the composition content of each element except carbon in the carbon-free residue, and correcting the detection result according to the ignition coefficient c to obtain the total composition content of the blast furnace wall condensed slag in step A);

[0015] The blast furnace wall condensed slag material of the present invention includes carbon-based materials, intermediate composite materials and ore-based materials. The carbon-based materials are blast furnace wall condensed slag materials with external dominant characteristics of certain coal-coke products, and are blast furnace wall condensed slag materials with a carbon-based mass content greater than 15%; the ore-based materials are blast furnace wall condensed slag materials with external dominant characteristics of certain ore-based products, and are blast furnace wall condensed slag materials with a carbon-based mass content less than 5%; the intermediate composite materials are blast furnace wall condensed slag materials with external dominant characteristics that are not obvious or difficult to distinguish, and are blast furnace wall condensed slag materials with a carbon-based mass content of 5 to 15%. In practical applications, the present invention needs to perform sample inspection and pre-batch processing on the blast furnace wall condensed slag material before deciding whether to perform fixed carbon and fixed sulfur analysis or infrared carbon and sulfur analysis on the blast furnace wall condensed slag material. Specifically, the appearance particle size and state of the blast furnace wall condensed slag material can be used to preliminarily judge whether it is a carbon-based material, a ore-based material or an intermediate composite material between the two, and preliminarily classify and place it. For example, the blast furnace wall condensed slag is classified and identified by visual inspection or hand twisting. When the carbon-based content is less than 5%, the hand-twisted sample will have obvious dominant characteristics of mineral-based materials, that is, it feels rough and turbid, has a sense of gravel, has no stickiness in the powder, and does not hang on the hand, and is intended to be classified as a mineral-based material; when the carbon-based content is greater than 15%, there will be obvious dominant characteristics of coal-coke-based materials, that is, it feels light and frivolous, has no sense of gravel, has a slightly sticky powder, and is black and hangs on the hand, and is intended to be classified as a carbon-based material; when the carbon-based content is between 5 and 15%, the above two characteristics cannot be clearly distinguished by visual inspection or hand twisting, or both characteristics are present, and it is intended to be classified as an intermediate composite material. Because different material bases will correspond to different detection steps later, and the subsequent experimental conditions will also be different, it is helpful to classify and batch the blast furnace wall condensed slag in advance to differentiate the experimental process and obtain the best detection plan.

[0016] The detection target of the present invention is to quickly detect the major and minor elements of the blast furnace wall condensed slag, namely the content of carbon, iron, silicon, calcium, magnesium, aluminum, sulfur, phosphorus, titanium, potassium, sodium, lead, zinc, arsenic and copper, and more specifically to quickly detect the corresponding major and minor components, including C, Fe, SiO2, CaO, MgO, Al2O3, S, P, TiO2, K2O, Na2O, Pb, Zn, As and Cu, a total of 15 components to be tested. Among all the 15 components to be tested, carbon is the most special one, because the source of carbon mainly comes from carbon-based materials such as coke in the charge, and the free carbon formed by the incomplete combustion of the carbon-based materials will seriously corrode the platinum-gold crucible for melting and sample preparation at high temperature, affecting the accurate measurement of the X-ray fluorescence instrument, so it needs to be detected separately and strictly removed. The other 14 elements can theoretically be detected by glass melting and film preparation-X-ray fluorescence method, but the detection effectiveness varies due to the accuracy of the instrument itself. Among them, the iron element needs to use cobalt as an internal standard, and set the attenuation when the feedback signal is strong to obtain more satisfactory detection accuracy. The six types of trace elements, potassium, sodium, lead, zinc, arsenic, and copper, have narrower detectable ranges than other element standard substances, and it is more difficult to obtain a more accurate measurement range under the same conditions. Another special one is sulfur, because sulfur generally exists in the form of sulfide in raw materials and is less corrosive. It can be included in the conventional elements for harmless glass melt detection; in theory, the sulfur content measured by the infrared carbon-sulfur analysis method and the sulfur content calculated by the fluorescence method should be very close in value and can be referenced and verified with each other.

[0017] The present invention first performs carbon determination and sulfur determination analysis or infrared carbon-sulfur analysis on the blast furnace wall condensed slag to obtain the carbon content and sulfur content of the blast furnace wall condensed slag. Specifically, the carbon-based material in the blast furnace wall condensed slag is subjected to carbon determination and sulfur determination analysis, the ore-based material in the blast furnace wall condensed slag is subjected to infrared carbon-sulfur analysis, and the intermediate composite material in the blast furnace wall condensed slag can be subjected to carbon determination and sulfur determination analysis or any one of infrared carbon-sulfur analysis. The carbon determination and sulfur determination analysis described in the present invention specifically refers to the analysis with reference to GB / T476-2008 "Determination Method of Carbon and Hydrogen in Coal" and GB / T214-2007 "Determination Method of Total Sulfur in Coal" or the use of a carbon determination and sulfur determination instrument to analyze the sample to be tested; in actual application, the present invention uses a carbon determination and sulfur determination instrument dedicated to coal coke to perform carbon-sulfur analysis on carbon-based materials or intermediate composite materials with obvious coal coke properties. The infrared carbon-sulfur analysis described in the present invention specifically refers to the analysis performed with reference to GB6730.61-2005 "Determination of carbon and sulfur content of iron ore - High frequency combustion infrared absorption method"; in practical applications, the present invention uses an infrared carbon-sulfur analyzer commonly used for ore samples and steel samples to perform carbon-sulfur analysis on ore-based materials or intermediate composite materials with obvious ore properties.

[0018] In the field of carbon measurement of iron-making furnace charges, there is generally a strict division between the selection of instruments corresponding to carbon-based materials and ore-based materials, and they cannot be completely mixed without distinction. The former has rich carbon bases and more impurities in the condensed mineral phase, which is more similar to coal coke products in nature. When measuring carbon, it is suitable for the carbon and sulfur determination instruments commonly used in coal coke products; the latter has mainly ore bases in the condensed mineral phase, with limited impurity losses, which is more similar to iron ore products in nature. When measuring carbon, it is suitable for the infrared carbon-sulfur instrument commonly used in iron ore products. Firstly, because carbon-based materials will produce more impurities and harmful gases at high temperatures, if infrared carbon-sulfur instruments are forced to be used for detection, it will cause greater damage to the instrument itself, accelerate the damage of the built-in components of the instrument and the failure of agents such as soda lime and magnesium perchlorate, and affect the detection performance of the equipment. Secondly, the density of carbon-based materials is relatively small, and the external volume is too large for the same mass as ore-based materials, which is not suitable for the operating environment of the infrared carbon-sulfur instrument micro-crucible. Third, the combustion performance of carbon-based materials is too strong, and often a small mass will produce excessive burning, which usually exceeds the set range of the infrared carbon-sulfur analyzer, resulting in over-limit inspection and inability to accurately display the value. Therefore, in inspection production, it is usually necessary to strictly distinguish between the carbon measurement of two materials with different properties. However, when faced with intermediate composite materials whose carbon-based and mineral-based characteristics are not obvious, it is generally believed that the base carbon content will not be too high, and the potential damage to the equipment is small. For this type of material, the infrared carbon-sulfur analyzer and the fixed carbon and sulfur analyzer can be used for simultaneous detection. When the infrared carbon-sulfur analyzer exceeds the range and cannot accurately display the data, it can be switched to the fixed carbon and sulfur analyzer for detection and then calibrated. Otherwise, the carbon result measured by the infrared carbon-sulfur analyzer can be used as the final result.

[0019] Furthermore, in the present invention, if a fixed carbon and fixed sulfur analysis is performed, the carbon content and sulfur content of the obtained blast furnace wall condensed slag need to be calibrated according to the carbon value calibration coefficient a and the sulfur value calibration coefficient a', respectively. The carbon value calibration coefficient a and the sulfur value calibration coefficient a' are the ratio of the carbon content (the ratio of the carbon content of the fixed carbon and fixed sulfur analysis to the carbon content of the infrared carbon and sulfur analysis) and the sulfur content (the ratio of the sulfur content of the fixed carbon and fixed sulfur analysis to the sulfur content of the infrared carbon and sulfur analysis) obtained by performing a fixed carbon and fixed sulfur analysis on the intermediate composite material and performing an infrared carbon and sulfur analysis, respectively. The calibration is specifically performed by dividing the carbon content result obtained by the fixed carbon and fixed sulfur analysis by the carbon value calibration coefficient a to obtain a proposed carbon analysis value; and dividing the sulfur content result obtained by the fixed carbon and fixed sulfur analysis by the sulfur value calibration coefficient a' to obtain a proposed sulfur analysis value. In the present invention, because different types of blast furnace wall condensed slag are detected by different inspection methods and inspection equipment, there must be generation differences between the data, and there are no conditions for horizontal comparison. Therefore, the carbon and sulfur detection data of the intermediate composite material that can be detected by both methods are selected, and the generation difference coefficients of the two methods for detecting the same material are calculated, which are defined as the carbon value correction coefficient a and the sulfur value correction coefficient a' respectively. The carbon and sulfur results of all carbon-based materials detected by the carbon and sulfur determination instrument are divided by the coefficient, and all are converted into the values ​​detected by the infrared carbon and sulfur instrument, which can basically eliminate the influence of the generation difference. This is mainly because: among all blast furnace wall condensed slag, non-carbon-based material types still account for the majority in quantity. Furthermore, the measurement accuracy of the infrared carbon-sulfur method is generally higher than that of the carbon and sulfur determination method.

[0020] After obtaining the carbon content of the blast furnace wall condensed slag, the present invention needs to estimate a reasonable burning sample amount for the blast furnace wall condensed slag according to the carbon content of the blast furnace wall condensed slag, select an appropriate burning scheme, and classify and burn it in an orderly manner until it is carbon-free under economical experimental conditions, so as to collect all carbon-free residues and calculate their burning coefficients. Because the present invention needs to calculate the burning coefficient, the particles must be returned to the warehouse after collecting the residues to avoid omissions, and the net weight must be weighed on the scale. This process must be careful and accurate, and the inner wall of the crucible must be carefully brushed clean with a brush to avoid dissipation during the process. The present invention adopts a normal burning scheme to burn the blast furnace wall condensed slag with a carbon content less than or equal to the carbon content of the intermediate composite material with the highest carbon content until it is carbon-free, and adopts a strict burning scheme to burn the blast furnace wall condensed slag with a carbon content higher than the carbon content of the intermediate composite material with the highest carbon value. The present invention determines the common burning scheme and the strict burning scheme with reference to the experimental conditions that the intermediate composite material with the highest carbon content in the blast furnace wall condensed slag can be burned to carbon-free. The burning scheme described in the present invention generally includes parameter information such as the configuration burning amount, the configuration crucible amount, the burning temperature, and the burning time; wherein the common scheme is specifically: for the blast furnace wall condensed slag with a carbon-based content of less than 15%, it is burned at 650~750℃ until it is carbon-free, specifically, it is burned at 650~750℃ for 3~5h with a configuration burning amount of 1.5~2.5g in an environment of 650~750℃; the strict scheme is specifically: for the blast furnace wall condensed slag with a carbon-based content greater than 15%, it is burned at 900~1000℃ until it is carbon-free, specifically, it is burned at 2.5~4.5g in an environment of 900~1000℃ for 10~14h. In practical applications, after the burning is completed, there are generally two standards for determining carbon-free: first, the overall color of the burned powder is white after cooling, and the inner bottom is checked to see if there is no obvious unburned material left; second, the powder is taken for infrared carbon-sulfur analysis, and the carbon content is measured to be no more than 10 ppm. In order to reduce the amount of verification in actual operation, the samples with the highest carbon value in the two-grade burning scheme, namely the intermediate composite material and the carbon-based material, can be selected for carbon-free verification. When the burned powder is sufficient, the infrared carbon-sulfur method verification is preferred, and when the powder is insufficient, the color identification verification is preferred. At the same time, since the burning time of the stricter scheme is longer, the number of samples in practice accounts for a smaller proportion. In order to reduce unnecessary waiting and speed up the process, it is recommended to give priority to burning the blast furnace wall condensed slag materials that need to implement the ordinary scheme, so that when the stricter scheme is implemented for other blast furnace wall condensed slag materials, the blast furnace wall condensed slag materials burned in the ordinary scheme can be simultaneously glass melted and sliced.

[0021] In practical applications, while the present invention classifies and burns the condensed slag of the blast furnace wall, it is necessary to separately calculate whether the current amount of sample placed in the burning can be collected after the burning to obtain a sufficient powder sample for melting and filming. Generally, the greater the carbon content, the less powder can be collected after burning, and the higher the configured burning amount. Among them, those with abnormally high carbon content represent carbon-based enrichment in the original sample, and there are more impurities such as ash volatiles. It is necessary to add more sample amounts in the subsequent gravity burning method, lay more crucibles, and appropriately increase the burning temperature and lengthen the burning time within the scope of its burning scheme to completely eliminate carbon-based impurities as soon as possible. At the same time, according to the carbon content obtained by the carbon and sulfur meter or the infrared carbon and sulfur meter, the minimum configured burning amount can also be roughly calculated to ensure that a residue sample of not less than 1 g can be obtained in the subsequent glass melting process (slightly higher than the actual demand of 0.7g, and the loss of powder should be taken into account). Here, the sample with the highest carbon content in the two burning schemes should be used as the reference target. The estimated method is that the burning amount minus the carbon percentage should be no less than 2 g (considering the various impurities other than carbon in the above standard). It is not ruled out that the carbon content of individual samples is extremely high, that is, after all samples are placed in the burning, the powder after burning is difficult to reach the minimum 0.7g sample weight required for normal melting. In this case, the lower limit of weighing can be set to 0.35g, that is, the half amount of the batch of samples is measured with a double dilution ratio, and then the fluorescence calibration coefficient b is added for calibration. After strict burning and carbon removal, the residue can be infinitely close to the iron ore base, and the conventional iron ore method should be used for subsequent detection by X-ray fluorescence spectroscopy.

[0022] The present invention should configure the burning scheme for each batch of samples of the blast furnace wall condensed slag material based on the principle of economic saving. The parameters should be configured once to test multiple batches of samples at the same time, put them into the furnace at the same time, and take them out of the furnace at the same time. In order to remove carbon and solidify it as much as possible, it is also necessary to comprehensively consider the existing laboratory conditions, reduce unnecessary waiting time and material waste, and speed up the experimental process. In certain embodiments of the present invention, the conditions of the burning scheme are summarized as shown in Table 1:

[0023] Table 1

[0024]

[0025] It should be noted that the weight lost by the burning method is not all carbon, and the two are not completely equivalent, but there is a strong positive correlation trend. In addition, the use of gravity burning method does not necessarily cause a reduction in the sample mass. In the case of low carbon base and high mineral phase, the burning reaction may oxidize the reducing elements in the mineral phase, and after absorbing oxygen in the air, it will cause the weight after burning to increase. This is a normal phenomenon and should be carefully distinguished in actual application.

[0026] After the present invention completes the burning of the blast furnace wall condensed slag, it is necessary to weigh it as soon as possible after it is cooled to room temperature to avoid moisture absorption by the sample and affect the accuracy of the result. Before collecting the residue sample, the burning coefficient c of the sample needs to be calculated synchronously and quickly. The burning coefficient of the present invention is the ratio of the mass of the carbon-free residue obtained after the burning of the blast furnace wall condensed slag in step A) to its mass before burning, and its value should be a number between 0 and 1 (in special cases, it will exceed 1), and at least four significant figures are retained. The burning coefficient values ​​of different types of blast furnace wall condensed slag are different, which reflects the specific differences between the coke residue and the mineral phase residue of the condensed wall slag sampled at different positions of the furnace body. The larger the carbon-based ratio, the more corresponding accumulated error factors, and the more uncertain the result. This value needs to be substituted into the product when the final calculation result is calculated, and the component result presented by the fluorescence spectrometer is reversed to calibrate the experimental data. When the sample has a large amount of base coke residue, most of its carbon-based mass is lost during burning, and the composition of the remaining residue is "highly concentrated" and needs to be multiplied by a lower coefficient to restore it to the actual form of the original sample; otherwise, it needs to be multiplied by a higher coefficient. In extreme cases, such as when the burning coefficient is calculated to be 1, the material can be regarded as full-ore phase wall slag and can be tested indiscriminately with reference to the iron ore test method.

[0027] According to the present invention, after different types of blast furnace wall condensed slag are burned to be carbon-free according to different burning schemes and the burning coefficient is calculated, the carbon-free residue obtained after burning needs to be subjected to glass melting film making-X-ray fluorescence spectrum detection to obtain the composition content of each element of the carbon-free residue except carbon. If the obtained carbon-free residue is sufficient for full X-ray fluorescence spectrum detection, the full X-ray fluorescence spectrum detection is performed to obtain the full X-ray fluorescence spectrum detection result of each element composition of the carbon-free residue; if the obtained carbon-free residue is not sufficient for full X-ray fluorescence spectrum detection, the half X-ray fluorescence spectrum detection is performed to obtain the half X-ray fluorescence spectrum detection result of each element composition of the carbon-free residue, and then the half X-ray fluorescence spectrum detection result is calibrated according to the fluorescence calibration coefficient b to obtain the proposed full X-ray fluorescence spectrum detection result of the carbon-free residue.

[0028] The full X-ray fluorescence spectrometry detection described in the present invention refers to the X-ray fluorescence spectrometry analysis result obtained by weighing the full mass material for glass melting and filming with reference to GB / T 6730.8-2023 "Determination of total iron and other multi-element content in iron ore by wavelength dispersive X-ray fluorescence spectrometry (cobalt internal standard method)", and the full mass is 0.4 g~0.8 g; the half X-ray fluorescence spectrometry detection refers to the X-ray fluorescence spectrometry analysis result obtained by weighing the half mass material for glass melting and filming as specified in the national standard; the half mass is half of the full mass. In certain embodiments of the present invention, the full X-ray fluorescence spectrometry detection is the X-ray fluorescence spectrometry analysis result obtained by weighing 0.7 g of material for glass melting and filming; the half X-ray fluorescence spectrometry detection is the X-ray fluorescence spectrometry analysis result obtained by weighing 0.35 g of material for glass melting and filming.

[0029] The fluorescence calibration coefficient b of the present invention is the ratio of the fluorescence intensity of each element of the intermediate composite material subjected to half-amount X-ray fluorescence spectrum detection and full-amount X-ray fluorescence spectrum detection. The reason for the existence of this coefficient is that it is not ruled out that some carbon-based materials have too little residue material after burning because the overall carbon base is too large. Even after all the samples are burned, the collected residue cannot meet the basic condition of the minimum material weighing weight required for the subsequent glass melting and film making for the full amount of X-ray fluorescence spectrum detection. In this case, the carbon-free residue after the intermediate composite material is burned needs to be subjected to full-amount X-ray fluorescence spectrum detection and half-amount X-ray fluorescence spectrum detection respectively to obtain the fluorescence calibration coefficient b. In the subsequent summary, the half-amount X-ray fluorescence spectrum detection results of all carbon-free residues detected by half-amount X-ray fluorescence spectrum are subjected to a proposed calibration according to the fluorescence calibration coefficient b, that is, the half-amount X-ray fluorescence spectrum detection result is divided by the fluorescence calibration coefficient b to obtain the proposed full-amount X-ray fluorescence spectrum detection result of each element of the carbon-free residue, and all the fluorescence test results obtained by half-amount weighing are pushed back to the fluorescence test results obtained by full-amount weighing to achieve the proposed calibration. The fluorescence intensity effectiveness of each element produced by the full-amount X-ray fluorescence spectrum detection result and the half-amount proposed full-amount X-ray fluorescence spectrum detection result calibrated with the fluorescence calibration coefficient b are basically consistent, and will not be repeated here.

[0030] In the present invention, the carbon-free residue obtained in step B) is subjected to glass melting film-X-ray fluorescence spectrum detection, and after obtaining the composition content of each element of the carbon-free residue except carbon, the detection result is corrected according to the burning coefficient c to obtain the total composition content of the blast furnace wall condensed slag material in step A). ​​The correction of the detection result according to the burning coefficient c is to multiply the composition content of each element of the carbon-free residue except carbon obtained by the burning coefficient c, and combine the corrected result with the carbon content obtained in step A to obtain the total composition content of the blast furnace wall condensed slag material in step A).

[0031] After obtaining the total element composition content of the blast furnace wall condensed slag in step A), the present invention further includes secondary correction of the iron element composition content and the sulfur element composition content in the total element composition content; wherein the secondary correction of the iron element composition content is specifically to chemically titrate the blast furnace wall condensed slag in step A) with potassium dichromate to obtain the corrected iron element composition content of the blast furnace wall condensed slag in step A), and replace the iron element composition content in the total element composition content with the corrected iron element composition content obtained; the secondary correction of the sulfur element composition content is specifically to replace the sulfur element composition content in the total element composition content with the sulfur content obtained in step A). ​​The present invention uses potassium dichromate to chemically titrate the blast furnace wall condensed slag with reference to "GB / T 6730.5-2022 Determination of the total iron content of iron ore by titration after titanium trichloride reduction".

[0032] In addition, in practical applications, after the X-ray fluorescence spectrum detection of step C) is performed in the present invention, it is also necessary to establish a linear regression curve suitable for the conventional detection range of each element except carbon based on various existing standard substances. The more refined the early line building process is, the higher the accuracy of the results obtained by the later detection of the sample. Because the condensed slag from the blast furnace wall is a mixture condensed under special conditions, some elements are easily enriched, and various components are possible. One of its elements is often not controlled by common sense conditions and suddenly jumps to exceed the limit. This situation is due to the current lack of experimental hardware and limited detection conditions. If there is no special need, the quantitative value of a single batch can be appropriately ignored, and only its macroscopic distribution trend can be observed. Otherwise, it is necessary to improve the experimental conditions, or use other methods for auxiliary verification.

[0033] In practical applications, the present invention can also use the matching degree of the sulfur content in the fluorescence spectrum detection result and the sulfur content obtained in step A, and whether the weighted value of all detectable elements reaches or approaches 100% as a simple verification condition to verify whether there are significant error factors in the process. For a single test, the systematic error may not be removed, but when the data sample size is sufficient, it is likely to satisfy the normal distribution, and all its data can be statistically analyzed to obtain a suitable judgment conclusion. Specifically, when the sampling position is known to be random and uniform, the blast furnace wall condensed slag material in step A) of more than 20 samples is detected by the detection method, and the weighted statistics of all element composition contents of the blast furnace wall condensed slag material in step A) obtained in step C) are included in the data normal distribution analysis to verify that its weighted data group should generally satisfy the normal distribution law; otherwise, it is necessary to examine whether there are significant error factors in the process and make a secondary judgment on the analysis data. The data normality distribution law of the present invention is that the weighted value of each element content of each blast furnace wall solidified slag obtained is in a bell-shaped distribution state at a certain mean value between 90% and 100%.

[0034] The present invention also provides an application of the above detection method in blast furnace condition diagnosis. Specifically, the blast furnace condition can be comprehensively compared and analyzed based on the result array of condensed slag on the blast furnace wall obtained by the detection, providing a judgment basis for the ironmaking department to study and diagnose the furnace condition, steadily extend the life of the blast furnace, and reduce costs and increase efficiency for new steel enterprises. DETAILED DESCRIPTION

[0035] The present invention discloses a method for detecting the elemental composition content of condensed slag of a blast furnace wall and its application. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters for implementation. It is particularly important to point out that all similar substitutions and modifications are obvious to those skilled in the art, and they are all considered to be included in the present invention. The method and application of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the method and application of this article without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.

[0036] The following preparations are made in the specific implementation manner of the present invention:

[0037] 1. The inspection equipment or utensils provided are:

[0038] Simultix12 X-ray fluorescence spectrometer (must have fixed or scanning channels for all elements to be tested);

[0039] CS-800 high-frequency infrared carbon-sulfur analyzer (with basic accessories such as porcelain crucible and flux);

[0040] Sande SDS616 carbon and sulfur determination instrument (with basic accessories such as fine porcelain boat);

[0041] AL104 electronic balance (accuracy 0.0001g);

[0042] SGM type high frequency constant temperature muffle furnace (relevant temperature parameters can be freely set);

[0043] TR-AUTO-BEAD-1000-M melting machine (with free temperature setting and crucible rocking and mixing function in the furnace);

[0044] A number of platinum-gold crucibles, composed of 95% by mass of platinum and 5% by mass of gold;

[0045] Several open square porcelain boats, with open surface size of 55 mm×25 mm (including basic accessories such as crucible racks).

[0046] 2. The other experimental conditions prepared are generally as follows:

[0047] GSB03-2019 series iron ore standard materials (total iron content is approximately 55%~65%) 10 pieces;

[0048] 5 pieces of YSBC28602-28610 series carbon and sulfur standard samples (the measurable range of carbon is approximately 0.01%-10%);

[0049] A number of other auxiliary standard samples besides the above-mentioned standard substances;

[0050] Cobalt powder mixed flux (composed of CoCO3 polymer preparation, used as internal standard for iron element in fluorescence analysis);

[0051] Anhydrous lithium tetraborate and anhydrous lithium carbonate, both analytically pure (flux for glass making);

[0052] 40% concentration potassium iodide solution (release agent).

[0053] 3. Determination method and equipment type:

[0054] The wavelength dispersive X-ray fluorescence instrument: the instrument is equipped with a fixed channel or a scanning channel, and can measure Fe-K α 、Si-K α The spectral lines of more than ten elements can meet the spectral line requirements of blast furnace inspection elements. The test accuracy of each spectral line meets the JJG810-1993 X-ray fluorescence instrument metrological verification technical specifications. Analysis power 5 kW; analysis current 50 mA, other measurement conditions refer to Table 2:

[0055] Table 2

[0056]

[0057] When establishing the corresponding working curve, it is recommended to select no less than 10 certified standard samples that can cover the content range of the analyzed sample. The samples contain the above elements, and the standard content of the notes is appropriately separated. Prepare the standard sample frits in sequence, input the content of the standard samples, measure the intensity of the analytical line under the set fluorescence instrument measurement conditions, and establish a regression model of the standard value to the measured intensity or intensity ratio. When regressing the working curve, regress the analytical spectral line intensity with the standard value, and use the single line mode.

[0058] Due to the limited number and coverage of certified standard samples, if the elements tested exceed the defined interval, there will be a large measurement uncertainty. For data results that fall within the coverage of the standard material, the correlation coefficient of the working curve should not be less than 0.95 during the first regression. If the regression correlation coefficient is too low, or the data results obtained by measuring the range too far, there will be a certain risk of segregation. On the basis of not increasing the experimental investment cost, it is recommended to ignore the absolute accuracy of a single indicator for such data. When the sample size is sufficient, observe its macroscopic change trend, or use statistical analysis methods to obtain relevant conclusions. If it is necessary to pay attention to this single indicator, it is necessary to introduce parallel experiments or add other methods to assist in verification.

[0059] The method for detecting condensed slag on the blast furnace wall of the present invention comprises the following steps:

[0060] 1) Sample inspection and pretreatment:

[0061] All samples sent for inspection are numbered and their appearance is checked after being unpacked one by one. First, determine whether each sample meets the basic requirements such as sample dryness, fine and uniform particle size, and no obvious impurities. The prepared samples must meet the sample preparation specifications, and the basic particle size should not be less than 0.125 mm.

[0062] Secondly, the texture of the samples is judged by appearance one by one to determine the carbon content of its mineral phase base, that is, to analyze whether the material is generally carbon-based, mineral-based, or an intermediate composite material with both characteristics. Whether a blast furnace wall condensed slag material is carbon-based or mineral-based, that is, whether its main component is carbon or other major elements, can be basically judged by visual inspection and hand twisting. Carbon-based materials are light and floating, and the powder hangs on the hand; mineral-based materials are heavy and turbid, and the powder does not hang on the hand. Here, based on the judgment conditions of whether the sample has black hanging fingers and obvious gravel feeling after hand twisting, the samples submitted for inspection are roughly divided into three batches: samples that are delicate, light and floating, and black hanging fingers are predicted to be carbon-based batches; samples that are heavy and turbid, do not hang on the hand, and have a gravel feeling are predicted to be mineral-based batches; those that have both characteristics or cannot be clearly judged can be classified as intermediate composite materials and put in a separate batch.

[0063] If it is pre-judged as a carbon-based material, it is necessary to check whether the sample quality is sufficient, which is generally considered to be no less than 20 g. If the sample quantity is obviously insufficient, you can contact the sample preparation department to appropriately increase the sample quantity to avoid insufficient samples after burning in the subsequent burning process, which will delay the subsequent inspection.

[0064] 2) Carbon and sulfur detection under different conditions

[0065] Before the experiment begins, it is necessary to check the instrument status and calibrate the instrument channels in real time with carbon and sulfur standard substances in the corresponding detection range to ensure that the experimental process is accurate and reliable. Carry out fixed carbon and fixed sulfur analysis on the pre-classified carbon-based materials, and infrared carbon and sulfur analysis on the ore-based materials. For intermediate composite materials of uncertain attribution, pick at least one batch for simultaneous fixed carbon and fixed sulfur analysis and infrared carbon and sulfur analysis to calculate the carbon value correction coefficient a and sulfur value correction coefficient a' for the two methods of determining carbon and sulfur (if multiple batches are tested, take a reasonable average). After all carbon and sulfur determinations are completed, record their carbon and sulfur contents by number, and divide the carbon and sulfur results of all the above-mentioned carbon-based materials detected by the fixed carbon and fixed sulfur instrument by the carbon value correction coefficient a and sulfur value correction coefficient a', and all are calculated into carbon and sulfur values ​​detected by the proposed infrared carbon and sulfur instrument. The above samples are sorted by their corrected carbon values, and the carbon value closest to 15% (i.e., the highest carbon content of the intermediate composite material) is determined as the dividing line for different burning schemes. For those with lower carbon values, the ordinary burning scheme is selected, and for those with higher carbon values, the stricter burning scheme is selected.

[0066] 3) Gravity burning method to remove carbon-based impurities;

[0067] In order to ensure the rapid progress of the experiment, samples with low carbon content are preferentially burned according to the ordinary file scheme. If conditions permit, it is recommended to select intermediate composite materials with high carbon content for parameter experimental identification of the burning scheme, otherwise at least the burning scheme parameters shown in Table 3 below shall be implemented. At the same time, the total weight of the sample before burning needs to be strictly weighed before burning. When performing the burning operation, open square porcelain boats are preferred, and the samples are made as thin as possible. When the carrying capacity of a porcelain boat is not enough to cover the entire sample, the number of square porcelain boats can be increased, and they can be arranged on the same crucible rack, the numbers are recorded, and they are placed in a muffle furnace with set parameters to ensure that a unified burning end point is obtained under the same standard. Generally, after the burning is completed, it is necessary to check the internal morphology of the sample to see if there is no obvious black carbon residue inside. If necessary, it is necessary to take samples of the burned residue for infrared carbon-sulfur analysis. The burned sample is measured by infrared carbon-sulfur method. The carbon analysis content is less than 10 ppm as the recognized burning end point.

[0068] The reference standards for the burning scheme are shown in Table 3:

[0069] Table 3

[0070]

[0071] If the ordinary burning scheme fails to completely burn to carbon-free, it can be classified as a stricter burning scheme to continue burning. When there is high-carbon value wall slag in the sample to be tested, it is necessary to more strictly identify it as carbon-free according to the above standards; otherwise, the conditions can be appropriately relaxed. At the same time, it is necessary to pay close attention to the collection of the post-burning residue of the sample, and it is advisable to collect more than 1 g of residue. In the worst case, the collected residue cannot be less than 0.35 g required for half-amount X-ray fluorescence spectrum detection.

[0072] After the burning is completed, it is necessary to weigh it as soon as possible after it cools to room temperature to prevent the sample from absorbing moisture and affecting the accuracy of the results. After collecting the residue sample, the total weight of the residue sample after burning needs to be weighed simultaneously, and the burning coefficient of each batch of samples is calculated and counted by the ratio of the residue after burning to the weight of the original sample. Under normal circumstances, the burning coefficient is defined as a number between 0 and 1 (in special cases it will be higher than 1), and at least four significant figures are retained.

[0073] 4) Glass melting samples and X-ray fluorescence spectrometer analysis;

[0074] Prepare 7.000 g of a mixed flux of lithium tetraborate and lithium carbonate in a mass ratio of 6:1, take 0.7000 g of the carbon-free residue sample after calcination, add 0.7000 g of cobalt powder mixed flux, mix thoroughly, add 5-10 mL of release agent, and place in a platinum-gold crucible.

[0075] Place the crucible in a melting machine that has been preheated to 1050°C, take it out after melting for 30 minutes, wait for it to cool to room temperature, and then demold it to obtain a glass sample. Check that there are no cracks, bubbles or crystals on the measuring surface of the sample.

[0076] Place the melted sheet in the sample box of the X-ray fluorescence analyzer, select the drawn working curve, enter the sample number, test in sequence, and wait for the analysis results to be displayed.

[0077] When the carbon-based content of a carbon-based material is too high, resulting in less than 0.7g of residue after burning, a half-weighing of 0.35g can be selected. At the same time, a fluorescence intensity comparison test of full weighing and half weighing is performed on the residue after burning of a batch of intermediate composite materials used in the experiment to obtain the ratio fluorescence calibration coefficient b of the two. In the final summary, the fluorescence results measured by half weighing are uniformly pushed back to the fluorescence results measured by the proposed full weighing.

[0078] 5) Calculate and verify the data based on the ignition coefficient.

[0079] Except for carbon, the instrument automatically displays the value of each measurement w The product of 0 and the burning coefficient is the proposed actual measured value of each component. w .

[0080] Among them, the carbon element has been calculated by the infrared carbon sulfur instrument or the carbon and sulfur determination instrument. The other major and minor elements except carbon are calculated by multiplying the total amount or the proposed total amount of X-ray fluorescence spectrum measurement results by the burning coefficient. At the same time, referring to GB / T16597-2019 "Methods for Analysis of Metallurgical Products - General Rules for X-ray Fluorescence Spectrometry Analysis" and GB6730.61-2005 "Determination of Carbon and Sulfur Content in Iron Ore - High Frequency Combustion Infrared Absorption Method", sulfur can be measured by either the infrared carbon sulfur instrument method or the glass melting film-X-ray fluorescence spectrometry method. The sulfur results obtained by the two methods can be compared horizontally to preliminarily determine whether the error of the entire experimental process is controllable.

[0081] In addition, when all the results of 15 elements appear, their weighting can be close to or reach 100% to determine whether the entire process is relatively reliable. It is generally believed that all weighted results exceeding 85% can meet the test requirements and the overall results are valid and usable. The causes of such test errors include but are not limited to system errors, process errors, weighing errors of ignition residues, X-ray fluorescence over-limit errors caused by single element transitions, and the possibility of unknown impurity elements in the original sample but not detected, etc.

[0082] The whole experiment generally takes about 6 hours to a day, and the cost-effectiveness of a single experiment on a certain sample is low. If conditions permit, a set of data should be added under the unified implementation standard, and a larger sample size should be used for statistical analysis of the data to better eliminate systematic errors and obtain more objective conclusions.

[0083] The present invention will be further described below in conjunction with embodiments:

[0084] Example 1

[0085] We received a sample A of condensed slag from a blast furnace wall. We twisted the powder by hand and found that it was light and floating. The powder was black and hung on our hands. There was no obvious granularity. We pre-judged that its base material belonged to carbon-based wall slag material. After verifying that its basic particle size was qualified, we put the entire sample on an electronic balance for weighing. It was found that the total weight of the sample bag was only about 2.5 g. Based on the fact that the residual amount of carbon-based materials after burning is generally 10%~50% (burning coefficient 0.1~0.5), it is estimated that the sample residue that can be collected in the end is likely to be less than the minimum 0.7g required for weighing glass melts. Therefore, we contacted the sample preparation department to increase the sample delivery quantity for this batch of samples. Otherwise, we can at least pre-judgment that the amount of residue collected by the sample will be higher than half of its amount, that is, 0.35g, otherwise the subsequent inspection will not be able to be carried out.

[0086] Take an appropriate amount of the sample into a fine porcelain boat and directly use it for the carbon determination and sulfur determination instrument that has been verified as a standard sample. The current carbon and sulfur results are pre-measured as C: 52.90%, S: 0.23% (the "%" symbol is omitted in the subsequent expression, the same applies to the fluorescence determination part, and the numerical expression is all percentage content). It is confirmed that the material is an obvious carbon-based material. Due to the low density of the material itself and the high calorific value per unit mass, it is not suitable for infrared carbon and sulfur instrument testing, so the material only has the results of the carbon determination and sulfur determination instrument. Although the detection range can still be roughly judged from the existing results, because the value and the value measured by the infrared carbon and sulfur instrument belong to different standards and different methods, they are not horizontally comparable in the summary data. In order to avoid the value being traceable, it is necessary to introduce the carbon value calibration coefficient a and the sulfur value calibration coefficient a' here to make horizontal corrections to the theoretical measurement results of the above two methods.

[0087] Correction data requires the introduction of an intermediate composite material that can conduct two experiments at the same time. The above samples are temporarily put aside, and an intermediate composite material B with the dominant characteristics of both mineral-based and carbon-based materials is selected from the sample group, and it is tested by a carbon determination and sulfur determination instrument and an infrared carbon-sulfur instrument respectively. The carbon values ​​of sample B were measured to be 5.39 and 6.78 respectively; the sulfur values ​​were 0.56 and 0.46 respectively. The average carbon value is within the range of the common sense judgment of the carbon content of intermediate composite materials (5-15), so the composite characteristics of this intermediate material are available. The carbon value calibration coefficient a of sample B is calculated to be 5.39 / 6.78=0.7956 (take four significant figures). This value indicates that under this experimental environment, the detection efficiency of the same sample using a carbon determination and sulfur determination instrument is about 80% of the detection efficiency of the infrared carbon-sulfur instrument. In theory, this characteristic value is applicable to all blast furnace wall condensed slag samples including samples A and B under the current environment. It is known that the infrared carbon sulfur meter is more effective in measuring carbon within its range, so it is necessary to push the carbon content measured above back to the level of carbon measured by the infrared carbon sulfur meter. That is, the carbon value of sample A is 52.90 / 0.7956, and the carbon value of sample A after calibration is 66.49. Similarly, the sulfur value calibration coefficient a' of sample A is 0.56 / 0.46=1.217, and the sulfur value after calibration is 0.23 / 1.217, which is 0.19.

[0088] Sort out the above two coefficients for future use. It should be noted that the carbon value calibration coefficient a and sulfur value calibration coefficient a' obtained from the above experiment are only applicable to the back-calculation of carbon and sulfur values ​​of explicit carbon-based materials that cannot be detected by infrared carbon-sulfur analyzer, and are only applicable under the current experimental conditions. It represents the ratio of the carbon and sulfur measuring capabilities of the carbon and sulfur analyzer to the infrared carbon-sulfur analyzer under the current experimental conditions. When the experimental conditions remain unchanged, the experiment only needs to be carried out once (its precision must be guaranteed, otherwise another set of parallel experiments on intermediate composite materials should be conducted and the average taken), and it can be used directly in subsequent calculations. If the two experiments are too long apart or the existing conditions have changed, it is recommended to recalculate the coefficients.

[0089] This coefficient is a ratio coefficient. Whether it is the fixed carbon and fixed sulfur method to the infrared carbon and sulfur method, or the infrared carbon and sulfur method to the fixed carbon and fixed sulfur method, the principle is the same. Once selected, the subsequent ratio relationship shall not be changed at will, otherwise it will cause serious inaccuracy of subsequent data.

[0090] According to common sense, when the carbon content is 66.49, the original sample is basically coke residue, and the sample needs a lot of carbon removal before subsequent experiments. Because the carbon-based material is large in volume and low in density, its net content is only about 0.6g when the square porcelain boat is filled. In the current laboratory environment, it is impossible to provide an unlimited number of porcelain boats of the same batch for burning. At most, only six can be configured (the maximum placement of an ordinary crucible rack). In order to ensure that sufficient residue samples are collected later, six square porcelain boats are equipped when using the gravity burning method, and six 0.600 g samples are weighed respectively. The strict burning environment is selected, and the sample is placed in a 950℃ muffle furnace for continuous burning for 12 hours. After the furnace is taken out, all the residues of 0.5443 g are collected. From the residue of 0.5443 g and the total amount of 3.600 g in the furnace, the theoretical burning coefficient c of the sample is calculated to be 0.5443 / 3.600=0.1512.

[0091] Since the collected residue of about 0.5 g is not enough to meet the minimum 0.7000 g full sample weight for glass melting and film making, but it meets the half sample weight of 0.35 g. In the case of obviously insufficient residue sample, in order to ensure the smooth progress of the experiment, 0.3500 g of the post-burning residue sample was accurately weighed from the residue of about 0.5 g, and mixed with lithium tetraborate, lithium carbonate and other solvents and cobalt powder (the dilution ratio increased from the original 1:10 to 1:20), placed in a platinum crucible, and the glass melting operation was completed in a 1050℃ melting furnace for 30 min. At the same time, the concept of fluorescence calibration coefficient b under half-weighing was introduced. It is necessary to weigh 0.7000g and 0.3500g of an intermediate composite material with a carbon range between (5~15) (such as sample B, or any other intermediate composite material) respectively, and carry out glass melting and film making-X fluorescence test under the same conditions. After demolding and cooling, they were placed in the pre-verified curve for fluorescence instrument measurement.

[0092] The intermediate composite material is used as the "standard sample" and the whole sample and half sample are weighed for melt filming. For each element except carbon and sulfur, the intensity of each element in the half sample is divided by the intensity of each element in the full sample to obtain the fluorescence calibration coefficient b of each element. The record list is shown in Table 4:

[0093] Table 4

[0094]

[0095] Fluorescence calibration coefficient refers to a temporary alternative method to ensure the follow-up of the experiment when the experimental conditions are insufficient. Because fluorescence analysis is a relative quantity analysis, when other experimental conditions remain constant, only one variable, the sample weight, is changed, and the intensity of the half-quantity analysis and the full-quantity analysis of the sample will show a strong positive correlation.

[0096] The fluorescence calibration coefficient b obtained in the above experiment represents the ratio of the intensity of each element measured by half-weighing to the intensity of each element measured by full-weighing under the current experimental conditions. In this experiment, it represents a set of values, not a single value, and each value is only effective for the current element. This value will be a decimal that is always less than 1 under the current definition. It is only applicable to the case where the carbon-based material is too light in density or the unit mass of the burned amount is too large, resulting in too little collected residue, making it impossible to weigh enough 0.7 g of residue sample. When half the amount of 0.35 g is poured into the glass melt for film making, the back-calculation of each element is only applicable under the current experimental conditions. When the experimental conditions remain unchanged, the experiment only needs to be carried out once, and it can be used directly in subsequent calculations. If the two experiments are too long apart or the existing conditions have changed, it is recommended to recalculate the coefficients.

[0097] Weigh half of the residue sample A to obtain the fluorescence intensity of each element in the sample and divide it by the fluorescence calibration coefficient b of each element to obtain the remaining component group values ​​as shown in Table 5:

[0098] Table 5

[0099]

[0100] In actual calculation, whether to multiply or divide by a coefficient depends on the standard for defining the fluorescence calibration coefficient b. In the present invention, because the half-analysis is defined as the numerator of the ratio and the full-analysis is defined as the denominator of the ratio, the ratio is always less than 1, so when measuring the half-analysis intensity of the sample, it is necessary to divide by the coefficient to obtain a larger full-analysis value. However, this is still only the component result of the residual powder. In order to obtain the result of the original blast furnace wall slag sample, the above results should be uniformly multiplied by the ignition coefficient c, that is, 0.1512, to obtain the fluorescence intensity data of each element of the original wall slag again. The statistics are shown in Table 6:

[0101] Table 6

[0102]

[0103] The above data, plus the carbon value of 66.49 obtained by the carbon sulfur analyzer, and the results of all the elements to be tested for sample a are summarized in Table 7:

[0104] Table 7

[0105]

[0106] Reading the above data horizontally, we find that the absolute contribution of the values ​​mainly comes from a few specific elements such as carbon, silicon, potassium, and zinc, and the contribution of other elements is very small. The larger the absolute amount of an element, the greater the error accumulation in the cumulative calculation. However, the horizontal relationship between the elements is relatively certain, and carbon obviously occupies a large position in it.

[0107] After reliability verification of all the above results, it was found that the weighted value of all elements was about 108, close to the theoretical value of 100. Here, it is judged that one of the main sources of error is the sudden change of the amount of zinc, which should be a trace amount, exceeding the range of stable and accurate detection defined by the standard material, resulting in a nonlinear relationship of fluorescence intensity in a certain excess section, but it was not found in the subsequent multiplication operation, resulting in the inaccuracy of some data. The evidence is that the zinc value of 177.13 obtained by the first self-test conversion is obviously not a correct value, but it is barely credible after being rounded off to 26.57 using the burning coefficient. Because the experiment involves multiple coefficient multiplication and cumulative calculations, the original absolute appearance of each value is difficult to trace after being repeatedly rounded off, but from the horizontal comparison of the above data groups, it can at least be interpreted that this is a pure carbon-based wall slag material with high carbon, high zinc and almost no iron remaining. From its numerical response results, corresponding to its sampling position in the blast furnace wall, it can be combined with the usual material usage habits to specifically study the reasons behind its formation of high zinc mechanism.

[0108] This experiment used all the coefficients mentioned in the invention, namely the carbon value calibration coefficient a, sulfur value calibration coefficient a', fluorescence calibration coefficient b, and ignition coefficient c. Multiple multiplication operations were performed during the data generation process. This is because this is an ultra-high carbon-based sample, which is a special case in sample inspection. In order to improve calculation efficiency, it is still recommended to use a pre-built Excel spreadsheet in the specific use process, embed the corresponding formulas and coefficients, so as to facilitate the subsequent data acquisition, storage and calculation.

[0109] At the same time, it can be observed that in this experiment, the sulfur value of 0.19 obtained by the infrared carbon-sulfur method using the carbon and sulfur determination instrument is exactly the same as the sulfur value of 0.19 obtained by multiplying the ignition coefficient using the X-ray fluorescence spectrometry method. This is an unexpected coincidence of the values ​​of a certain element determined under two completely different standards and different methods. Perhaps there are accidental factors, but at least it shows that the experimental process control is acceptable.

[0110] Example 2

[0111] We received a sample of blast furnace wall condensed slag material C. We pinched its powder and found that it was black and sticky, with a medium color and a distinct sense of gravel. We pre-judged that it was an intermediate wall slag material. It is not clear whether it is mainly carbon-based or mineral-based. We confirmed that its basic particle size is qualified.

[0112] Take an appropriate amount of the sample into a porcelain crucible, and first use it for high-temperature infrared carbon-sulfur instrument inspection. By observing the carbon peak waveform state in the computer, determine whether the current sample amount is excessive. If the carbon channel shows an obvious peak and then falls back quickly, it proves that the carbon element in the sample has been completely burned and the current sample amount is available; if the carbon channel always rises without a peak and then stops, it proves that too much sample is weighed at one time, exceeding the upper limit of the system inspection, and it is necessary to reduce the amount appropriately before retesting. If the carbon peak still does not appear when the amount is reduced to a very small amount, it can be preliminarily judged that the carbon base exceeds the amount and is not suitable for infrared carbon-sulfur instrument inspection. Use a fixed carbon and fixed sulfur instrument for inspection instead, and refer to Example 1 for data calculation of infrared carbon-sulfur instrument and fixed carbon and fixed sulfur instrument.

[0113] In this experiment, when the sample amount was reduced, an obvious carbon peak appeared on the screen and then fell back. After the instrument completed the integration, the current carbon and sulfur results were displayed as C: 7.85, S: 5.68.

[0114] The carbon value of 7.85 is within the judgment range of intermediate composite materials (5-15), which confirms that the sample belongs to the intermediate composite material. It is predicted that its carbon-based impurities are not high and the weighing can be normalized. When using the gravity calcination method, a square porcelain boat is equipped, 2.000 g of sample is accurately weighed, a normal calcination environment is selected, and it is placed in a 750℃ muffle furnace. Continuously calcined for 3 hours, and all the residues of about 1.6 g are collected after the furnace is taken out. From the residue of 1.6000 g and the total weight of 2.000 g, the theoretical calcination coefficient c of the sample is calculated to be 1.600 / 2.000=0.80.

[0115] 0.7000 g of the fired sample was accurately weighed from the 1.6 g residue, and the mixture was fully mixed with lithium tetraborate, lithium carbonate and other solvents and cobalt powder, and placed in a platinum crucible. The glass fusing operation was completed in a 1050°C melting furnace for 30 min. After demolding and cooling, the sample was placed in a pre-verified curve for fluorescence measurement. The remaining component group values ​​were obtained as shown in Table 8:

[0116] Table 8

[0117]

[0118] The above results are uniformly multiplied by the ignition coefficient of 0.8 to obtain the fluorescence intensity of each element of the original wall slag, and the carbon value measured by the infrared carbon-sulfur instrument is added, and the results are summarized as shown in Table 9:

[0119] Table 9

[0120]

[0121] Reading the above data horizontally, we find that the absolute contribution of the values, in addition to carbon, mainly comes from several conventional elements such as iron, sulfur, silicon, calcium, and aluminum. Its mineral phase composition is close to the composition distribution of low-grade iron ore, but with the participation of some carbon elements. Since most carbon and volatile impurities have been basically removed during burning, the remaining can be processed according to the iron ore glass melting film making method. This shows that as long as it is a non-high-carbon-based intermediate wall slag material, its characteristics will still be more inclined to the ore-based wall slag material.

[0122] The above data can be used to analyze and judge the situation of the blast furnace wall where the sample is located. After testing a large number of samples, a more accurate analysis of the entire blast furnace wall can be obtained. If there are more stringent requirements for the analysis results, the obtained results can be corrected twice; because there has always been a set of economical and convenient chemical testing methods in the laboratory for the precise measurement of iron elements, after confirming that the base carbon base is not high and does not affect the color change of the observation process, the initial sample can be chemically titrated by the potassium dichromate method with acid dissolution to perform lateral auxiliary verification of the data.

[0123] Chemical titration is an absolute quantity method, and the result is not affected by external factors. After chemical titration of the sample, the absolute amount of iron in the sample was measured to be 50.35. This value can directly replace 42.49 in the original table. Similarly, the sulfur value of 5.68 measured by the infrared carbon sulfur instrument can also be used to replace 5.24 in the original table. After sorting out the replacement data, Table 10 is obtained.

[0124] Table 10

[0125]

[0126] The cumulative weighted value of all elements in this group after replacement after full analysis is 93.51, which is still different from the theoretical value of 100, but within an acceptable range. In this way, the overall arrangement and composition of the elements are relatively obvious. This is a piece of ferroxene phase wall slag that has melted some carbon-based impurities. Its performance has the characteristics of both carbon-based and mineral-based, and it belongs to the intermediate composite material type. The second highest element is calcium, indicating that there may be some lime flux residues in the base. Sulfur is particularly noteworthy, with a sulfur value of 5.24, which is significantly higher than previous common sense. Combined with the sampling position of the material in the blast furnace wall, it is possible to specifically analyze why there is more sulfur enrichment in its state.

[0127] Since the accuracy of the results measured by the absolute method has a higher priority than the results measured by the relative method, if a clear result measured by the absolute method appears, it can directly replace the relative result in the original table, and the data set can be further corrected for a second time. In this experiment, chemical titration of iron and infrared carbon-sulfur method are both absolute methods. The directly measured iron, carbon, and sulfur values ​​are far more credible than the theoretical result of the relative value measured by fluorescence analysis multiplied by the ignition coefficient multiplied by the relative coefficient. If there are similar methods or conditions for other elements, they can also be modified and cited. Whether or not to do everything depends mainly on the client's requirements for data accuracy. Sometimes this correction may be very small, and sometimes it can greatly make up for the original calculation error. In the case of limited overall energy, it is recommended to replace the absolute detection of individual quantities with more relative detection to obtain clearer data statistical laws on big data.

[0128] Embodiments 3 to 8

[0129] We collected six representative wall slag samples from the carbon brick layer of the blast furnace hearth, 8.8 m below the residual iron area, 500-600 mm from the center line of the iron mouth, 7 m above the residual iron eye, 1 m from the cooling wall at 7 m above the cooling wall, and the tuyere condensation area, respectively, and recorded them as sample 1. # ~6 # As Examples 3 to 8, the full analysis results were calculated and summarized in the above manner, as shown in Table 11. Table 11 is a data table of the measured values ​​of the major and minor components in six types of blast furnace wall condensed slag:

[0130] Table 11

[0131]

[0132] In the above table, the values ​​marked with * are theoretically more accurate and are ultimately adopted in the weighted calculation. Among them, carbon, sulfur, and total iron elements all have the problem of cross-verification of multiple methods. In the first and second rows of the above elements in the table, carbon refers to the values ​​measured by the fixed carbon and fixed sulfur method and the infrared carbon and sulfur method respectively; sulfur refers to the fluorescence test value multiplied by the burning coefficient and the value measured by the infrared carbon and sulfur method (or the fixed carbon and fixed sulfur method is replaced by the infrared carbon and sulfur method); iron refers to the fluorescence test value multiplied by the burning coefficient and the value verified by the potassium dichromate titration method (chemical method). They are listed here for easy comparison. When using, if there are more stringent requirements, it is recommended to directly use the absolute value measured in the second row, which is closer to the theoretical value, to replace the relative value measured in the first row, in order to obtain more accurate data presentation.

[0133] From the big data in Table 11, it can be seen that in the control experiment using the secondary correction, all the data revisions are without exception closer to the 100% theoretical value. This shows that in the relative method of fluorescence detection, there will inevitably be error accumulation in the cumulative calculation process of multiple coefficients. For individual data, the absolute quantity test method can be used to appropriately supplement and correct the original data set (feasible, but not necessary). In addition, among the six groups of samples randomly selected above, four batches had cumulative weighted values ​​less than 100%, and two batches had cumulative weighted values ​​greater than 100%, which generally showed a trend of half-and-half differentiation. With the support of more samples for data statistics, it will be more clearly found that the weighted values ​​of all elements will appear in the form of a normal distribution near (90-100)%.

[0134] The upper and lower limits and interval values ​​of the process parameters (such as temperature, time, etc.) of the present invention can all realize the present method, and the embodiments are not listed one by one here. The contents not described in detail in the present invention can all be adopted from the conventional technical knowledge in the field.

[0135] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for detecting the elemental composition content of blast furnace wall condensed slag, characterized in that: The following steps are involved: A) Carry out carbon and sulfur determination analysis or infrared carbon and sulfur analysis on the blast furnace wall condensed slag to obtain the carbon content and sulfur content of the blast furnace wall condensed slag; The blast furnace wall condensed slag material includes a carbon-based material, a mineral-based material and an intermediate composite material, wherein the carbon-based material is subjected to a fixed carbon and fixed sulfur analysis, and the mineral-based material is subjected to an infrared carbon and sulfur analysis; the intermediate composite material is subjected to either a fixed carbon and fixed sulfur analysis or an infrared carbon and sulfur analysis; If a fixed carbon and fixed sulfur analysis is performed, the obtained carbon content and sulfur content need to be calibrated according to the carbon value calibration coefficient a and the sulfur value calibration coefficient a' respectively; The carbon value calibration coefficient a is the ratio of the carbon content in the analysis results obtained by performing a fixed carbon and fixed sulfur analysis on the intermediate composite material and performing an infrared carbon and sulfur analysis; The sulfur value calibration coefficient a' is the ratio of the sulfur content in the analysis results obtained by the fixed carbon and fixed sulfur analysis and the infrared carbon and sulfur analysis of the intermediate composite material; B) burning the blast furnace wall condensed slag obtained in step A) until it is carbon-free according to the carbon content of the blast furnace wall condensed slag obtained in step A), and collecting all carbon-free residues; C) subjecting the carbon-free residue obtained in step B) to glass melting film-X-ray fluorescence spectrum detection to obtain the composition content of each element of the carbon-free residue except carbon, and correcting the composition content of each element of the carbon-free residue except carbon according to the burning coefficient c to obtain the total composition content of the blast furnace wall condensed slag material in step A); the burning coefficient c is the ratio of the mass of the carbon-free residue obtained after the calcination of the blast furnace wall condensed slag material in step A) to its mass before calcination; The carbon-based material is a blast furnace wall condensed slag material having the external dominant characteristics of a coal-coke product, and is a blast furnace wall condensed slag material having a carbon-based mass content greater than 15%; The ore-based material is blast furnace wall condensed slag material having the external dominant characteristics of ore-based products, and is blast furnace wall condensed slag material having a carbon-based mass content of less than 5%; The intermediate composite material is a blast furnace wall condensed slag material whose external dominant characteristics are not obvious or difficult to distinguish, and is a blast furnace wall condensed slag material with a carbon-based mass content of 5% to 15%.

2. The method for detecting the element composition content of blast furnace wall condensed slag according to claim 1, characterized in that: Step B) is specifically: For blast furnace wall condensed slag with a carbon-based mass content of less than 15%, burn it at 650-750℃ until it is carbon-free; For blast furnace wall condensed slag with a carbon-based mass content greater than 15%, it is burned at 900~1000℃ until it is carbon-free.

3. The method for detecting the element composition content of blast furnace wall condensed slag according to claim 2, characterized in that: Step B) is specifically: For blast furnace wall condensed slag with a carbon-based mass content of less than 15%, burn it at 650-750℃ for 3-5 hours; For blast furnace wall slag with a carbon-based mass content greater than 15%, it is calcined at 900~1000℃ for 10~14 hours.

4. The method for detecting the element composition content of blast furnace wall condensed slag according to claim 1, characterized in that: Step C) specifically comprises: after burning the blast furnace wall condensed slag material in step A), if the obtained carbon-free residue is sufficient for full X-ray fluorescence spectrum detection, full X-ray fluorescence spectrum detection is performed to obtain full X-ray fluorescence spectrum detection results of each element composition of the carbon-free residue; If the obtained carbon-free residue is not sufficient for full X-ray fluorescence spectrum detection, a half X-ray fluorescence spectrum detection is performed to obtain a half X-ray fluorescence spectrum detection result of each element composition of the carbon-free residue, and then a proposed calibration is performed on the obtained half X-ray fluorescence spectrum detection result according to the fluorescence calibration coefficient b to obtain a proposed full X-ray fluorescence spectrum detection result of each element of the carbon-free residue; The fluorescence calibration coefficient b is the ratio of the fluorescence intensity of each element of the intermediate composite material when the half-dose X-ray fluorescence spectrum is detected and the full-dose X-ray fluorescence spectrum is detected.

5. The method for detecting the element composition content of blast furnace wall condensed slag according to claim 4, characterized in that: The full amount X-ray fluorescence spectrum detection is specifically to carry out glass melting and film making by weighing the full amount mass of the carbon-free residue, and then carry out X-ray fluorescence spectrum detection on the prepared glass melting and film making to obtain the full amount X-ray fluorescence spectrum detection result of the carbon-free residue; the full amount mass is 0.4 g to 0.8 g; The half-mass X-ray fluorescence spectroscopic detection is specifically carried out by weighing half the mass of the carbon-free residue to carry out glass melting and film making, and then carrying out X-ray fluorescence spectroscopic detection on the prepared glass melting and film making to obtain the half-mass X-ray fluorescence spectroscopic detection result of the carbon-free residue; the half-mass is half of the full mass.

6. The method for detecting the element composition content of blast furnace wall condensed slag according to claim 1, characterized in that: In step C), after obtaining the total element composition content of the blast furnace wall condensed slag in step A), the process further includes performing a secondary correction on the iron element composition content and the sulfur element composition content in the total element composition content; A secondary correction is performed on the iron element composition content, specifically, potassium dichromate is used to chemically titrate the blast furnace wall condensed slag in step A), to obtain a corrected iron element composition content of the blast furnace wall condensed slag in step A), and the iron element composition content in the total element composition content is replaced by the obtained corrected iron element composition content; The sulfur element composition content is corrected for the second time, specifically, the sulfur element composition content in the total element composition content is replaced by the sulfur content obtained in step A).

7. The method for detecting the element composition content of blast furnace wall condensed slag according to claim 1, characterized in that: Under the condition that it is known that the sampling positions are random and uniform, when the blast furnace wall condensed slag of more than 20 samples in step A) is detected by the detection method of the elemental composition content of the blast furnace wall condensed slag, all the elemental composition contents of the blast furnace wall condensed slag of step A) obtained in step C) are weighted statistically analyzed and included in the data normal distribution analysis to verify that the weighted data group sequence should generally satisfy the normal distribution law; otherwise, it is necessary to examine whether there are significant error factors in the process and make a secondary judgment on the analysis data.

8. The method for detecting the element composition content of blast furnace wall condensed slag according to claim 7, characterized in that: The normal distribution law of the data is that the weighted values ​​of the content of each element of each batch of blast furnace wall solidified slag obtained are in a bell-shaped distribution pattern with a certain mean value between 90% and 100%.

9. Application of the method for detecting the element composition content of blast furnace wall condensed slag as described in any one of claims 1 to 8 in blast furnace condition diagnosis.

Citation Information

Patent Citations

  • Method for determining carbon content in slag fluxing agent

    CN106706549A

  • Method of iron ore material classification judgment

    CN109047024A