Blood-compatible polyester elastomer and preparation method thereof
By introducing γ-polyglutamic acid into the side chain of the polyester elastomer to form a stable hydration layer, the coagulation problem of polyester elastomer during blood contact is solved, and efficient anticoagulation and antibacterial properties are achieved, improving the Its blood compatibility has expanded its application scope.
Patent Information
- Application Number
- CN202410963871.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-18
AI Technical Summary
Existing polyester elastomers are prone to cause blood coagulation when in contact with blood, and anticoagulants are easily lost, with poor compatibility, making it difficult to meet the blood compatibility requirements of medical devices.
By introducing gamma-polyglutamic acid into the side chains of the polyester elastomer, using transesterification reaction and click chemical reaction, a hemocompatible polyester elastomer with anticoagulant and antibacterial properties is formed, using polyethylene glycol and Low molecular weight gamma-polyglutamic acid forms a stable hydration layer, enhancing the stability and hemocompatibility of the material.
It achieves excellent anticoagulant performance, low hemolytic toxicity and high antibacterial rate of polyester elastomers, extends the anticoagulation time, improves the hemocompatibility of the material, and expands its application range in medical devices.
Smart Images

Figure SMS_6
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyester elastomers, and in particular to a blood-compatible polyester elastomer and a preparation method thereof. Background Art
[0002] In recent years, polymer materials have been increasingly used in medical devices that come into contact with human blood and tissues due to their excellent mechanical properties and mechanical durability. However, when the surfaces of these medical devices come into contact with blood, the foreign body reaction of the blood can cause blood coagulation, which eventually leads to the formation of thrombi. Excellent blood compatibility has become a basic requirement for cardiovascular medical devices, and good blood compatibility means that after the material comes into contact with blood, it does not cause platelet adhesion activation, does not induce coagulation, hemolysis, and does not induce immune activation, so that the blood maintains a normal flow state and reflects normal physiological functions. By modifying polymer materials, the blood compatibility of the material can be effectively improved, thereby meeting a wide range of clinical application requirements.
[0003] Polyester elastomers have been widely used in the fields of automotive parts, hoses, cables and wires, electronic appliances, industrial products, stationery and sports goods, etc. due to their high toughness and strength, good resilience, impact resistance, creep resistance, cold resistance, bending fatigue resistance, oil resistance, chemical and solvent resistance, etc. However, there is little research on polyester elastomer materials with good blood compatibility. Summary of the invention
[0004] The technical problem to be solved by the present invention is: to overcome the shortcomings of the prior art, to provide a blood-compatible polyester elastomer and a preparation method thereof, to introduce γ-polyglutamic acid into the side chain of the polyester elastomer, to solve the problems of easy loss of anticoagulants through physical adsorption and poor compatibility, so that the polyester elastomer has excellent anticoagulant properties, low hemolytic toxicity, high antibacterial rate, and can be used in medical devices that come into contact with blood or tissue.
[0005] The technical solution of the present invention is:
[0006] In one aspect, the present invention provides a method for preparing a blood-compatible polyester elastomer, comprising the following steps:
[0007] S1 uses aromatic dibasic acid dimethyl ester, allyl malonate dimethyl ester, aliphatic diol and polyethylene glycol as raw materials, adds catalyst and antioxidant to carry out ester exchange reaction and polycondensation reaction to obtain side chain olefin-containing polyester elastomer;
[0008] S2 immerses the side chain olefin-containing polyester elastomer in an organic solvent containing thiolated γ-polyglutamic acid, and in the presence of a photoinitiator and under ultraviolet light irradiation, a thiol-ene click chemical reaction occurs to prepare a blood-compatible polyester elastomer.
[0009] The present invention introduces γ-glutamic acid into the side chain of the polyester elastomer, which can introduce the required side chain function while maintaining the stability of the main polymer structure. Compared with introducing it into the main chain of the polyester elastomer, the change of the side chain often does not significantly change the conformation and arrangement of the polymer main chain, and has little effect on the physical and mechanical properties of the polyester elastomer.
[0010] Preferably, in step S1, the aromatic dibasic acid dimethyl ester is one or two of dimethyl terephthalate, dimethyl phthalate, dimethyl isophthalate, dimethyl biphenyl dicarboxylate and dimethyl 2,6-naphthalene dicarboxylate; the aliphatic diol is one or two of ethylene glycol, 1,3-propylene glycol and 1,4-butanediol.
[0011] Preferably, in step S1, the number average molecular weight of polyethylene glycol is 400-6000 g / mol; the molar ratio of aromatic dibasic acid dimethyl ester to aliphatic diol is 1:(1.2-1.8); allyl malonate dimethyl ester accounts for 5-15% of the total mass of dimethyl ester; and the mass ratio of aromatic dibasic acid dimethyl ester to polyethylene glycol is (0.25-4):1.
[0012] Preferably, in step S1, the catalyst is one or two of zinc acetate, magnesium acetate, antimony trioxide, antimony glycol, dibutyltin oxide, stannous octoate, tetrabutyl titanate and tetraisopropyl titanate, and the added amount is 0.01-0.1% of the total mass of the raw materials.
[0013] Preferably, in step S1, the antioxidant is one or two of antioxidant 1010, antioxidant 1098, antioxidant 168, antioxidant 1076 and antioxidant 1330, and the added amount is 0.1-1% of the total mass of the raw materials.
[0014] Preferably, in step S1, the transesterification reaction temperature is 180-210°C, the reaction time is 0.5-2h; the polycondensation reaction temperature is 230-260°C, the reaction time is 2-6h, and the vacuum degree is <100Pa.
[0015] Preferably, in step S2, the preparation method of thiolated γ-polyglutamic acid is: adding 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride to 2-(N-morpholino)ethanesulfonic acid (MES) buffer containing γ-polyglutamic acid and N-hydroxysuccinimide (NHS), activated for 5-90 minutes, then L-cysteine hydrochloride dissolved in 2-(N-morpholino)ethanesulfonic acid buffer was added dropwise, the pH value was adjusted to 4-7, and the reaction was carried out at room temperature with nitrogen protection and light protection for 2-24 hours. After dialyzation, lyophilization was performed to obtain a white powder, which is thiolated γ-polyglutamic acid.
[0016] Preferably, the molecular weight of γ-polyglutamic acid is 5000-100000 Daltons, the concentration of 2-(N-morpholino)ethanesulfonic acid buffer containing γ-polyglutamic acid is 5-20 g / L, the concentration of 2-(N-morpholino)ethanesulfonic acid buffer containing L-cysteine hydrochloride is 10-40 g / L, the molar ratio of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride to N-hydroxysuccinimide is (1-2):1, and the molar ratio of carboxyl, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride to L-cysteine hydrochloride in γ-polyglutamic acid is 1:(1-2):(1-2).
[0017] Preferably, the ratio of the mass percentage of thiolated γ-polyglutamic acid in the side chain olefin-containing polyester elastomer to the mass percentage of allyl dimethyl malonate in dimethyl ester is (1-1.5):1; the photoinitiator is 2-hydroxy-2-methyl-1-phenylacetone, benzoin dimethyl ether, benzophenone, phenyl (2,4,6-trimethylbenzoyl) phosphate lithium salt or 4-dimethylaminobenzoic acid ethyl ester, and the added amount is 0.5-3% of the total mass of the raw materials in step S2; the organic solvent is tetrahydrofuran, acetonitrile, N-methylpyrrolidone, dimethyl sulfoxide or N,N-dimethylformamide; the ultraviolet light irradiation time is 0.1-4h.
[0018] On the other hand, the present invention provides a blood-compatible polyester elastomer prepared by the above-mentioned method for preparing a blood-compatible polyester elastomer.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] 1. The polyester elastomer raw material of the present invention adopts polyethylene glycol, which can form a hydration layer through hydrogen bonds, so that the polyester elastomer has anti-adhesion and anti-coagulation properties; and the low molecular weight γ-polyglutamic acid is selected to form a hydration layer with higher density and tighter adsorption through the electrostatic effect of carboxyl and amino groups, which greatly improves the stability of the base material, thereby avoiding the problem of short-lasting anti-coagulation effect during the use of polymer materials.
[0021] 2. The present invention is based on polyester elastomer and introduces γ-polyglutamic acid on the side chain through click chemistry. The free carboxyl groups on the side chain can effectively reduce the adhesion of platelets or bacteria to the surface of the material, and has both anticoagulant and antibacterial properties, low hemolytic toxicity, and good blood compatibility. DETAILED DESCRIPTION
[0022] In order to enable persons skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention.
[0023] The various chemical reagents and chemicals mentioned in the embodiments of the present invention are all known and commonly used chemical reagents and chemicals in the prior art unless otherwise specified. The experimental methods in the embodiments of the present invention without specifying specific conditions are selected according to conventional methods and conditions or according to the product specifications.
[0024] The testing method in the embodiment of the present invention is as follows:
[0025] Hardness: Test according to the standard "GB / T 2411-2008 Determination of indentation hardness (Shore hardness) of plastics and hard rubber using a hardness tester". Put the hardness tester pressure seat in close contact with the sample for 3 seconds and then take the reading.
[0026] Recalcification time: 5mL rabbit blood and 3.8wt.% trisodium citrate aqueous solution were prepared into fresh anticoagulated blood in a volume ratio of 9:1; the above fresh anticoagulated blood and 0.9wt.% NaCl aqueous solution were prepared into diluted rabbit blood in a volume ratio of 1:1.25, and then centrifuged at 1000r / min for 10min, and the supernatant was taken as plasma for standby. The materials prepared in each embodiment and comparative example were cut into 0.2cm×0.2cm strips after injection molding, placed in a 0.9wt.% NaCl aqueous solution and soaked for 24h, then moved to a test tube, and then 0.2mL plasma and 0.2mL CaCl2 aqueous solution with a concentration of 0.025mol / L were added, placed in a 37℃ constant temperature water bath, and the stopwatch was used for timing. The test tube was gently shaken to mix the CaCl2 aqueous solution and the supernatant evenly. Three parallel samples were set for each group. When a white fibrous substance appeared in the test tube, the stopwatch was stopped, and the recalcification time was obtained. The recalcification time can reflect the anticoagulant activity. The longer the recalcification time, the better the anticoagulant activity.
[0027] Hemolysis rate: The test was conducted according to the standard “YBB00032003-2015 Hemolysis Test Method”, and the test blood was fresh rabbit blood.
[0028] Antibacterial rate: The test was conducted in accordance with the standard "GB / T 31402-2015 Plastics - Test method for antibacterial properties of plastic surfaces", and the test bacteria was Staphylococcus aureus (ATCC 6538P).
[0029] Example 1
[0030] The preparation method of the blood-compatible polyester elastomer of this embodiment comprises the following steps:
[0031] 1) Preparation of thiolated γ-polyglutamic acid
[0032] 20 g of γ-polyglutamic acid (molecular weight 50,000 Daltons) was dissolved in 1300 mL of MES buffer, and then 44.6 g of and 26.8 g of NHS, activated at room temperature for 30 min; then 24.4 g of L-cysteine hydrochloride dissolved in 610 mL of MES buffer was added dropwise, 0.1 M HCl solution was added to adjust the pH value to 5, and then nitrogen was protected from light at room temperature for 12 h, and then lyophilized after dialyzation to obtain a white powder, which is thiolated γ-polyglutamic acid.
[0033] 2) Preparation of polyester elastomers containing olefins in side chains
[0034] 3 kg of dimethyl terephthalate, 0.3 kg of dimethyl allylmalonate, 1.9 kg of 1,4-butanediol, and 2 kg of polyethylene glycol (M n =2000g / mol), 2.4g of tetrabutyl titanate, 2g of magnesium acetate and 16g of antioxidant 1098 were added into the reactor, and the temperature was raised to 180°C under nitrogen protection for ester exchange reaction. After 2h of reaction, the polymerization temperature was raised to 240°C, and polycondensation was carried out under a high vacuum of less than 100Pa for 4h to obtain a side chain olefin-containing polyester elastomer.
[0035] 3) Preparation of blood-compatible polyester elastomer
[0036] 1 kg of the side chain olefin-containing polyester elastomer was immersed in a dimethyl sulfoxide solution containing 90 g of thiolated γ-polyglutamic acid and 10 g of benzoin dimethyl ether, then irradiated with an ultraviolet lamp (λ = 365 nm) for 0.3 h, washed with ethanol to remove the remaining reactants, and dried in an oven to obtain a blood-compatible polyester elastomer.
[0037] Example 2
[0038] The preparation method of the blood-compatible polyester elastomer of this embodiment comprises the following steps:
[0039] 1) Preparation of thiolated γ-polyglutamic acid
[0040] 20 g of γ-polyglutamic acid (molecular weight 5000 Dalton) was dissolved in 1000 mL of MES buffer, and then 59.4 g of and 23.8 g of NHS, activated at room temperature for 5 min; then 36.6 g of L-cysteine hydrochloride dissolved in 1850 mL of MES buffer was added dropwise, 0.1 M HCl solution was added to adjust the pH value to 4, and then nitrogen was protected from light at room temperature for 2 h, and then lyophilized after dialyzation to obtain a white powder, which is thiolated γ-polyglutamic acid.
[0041] 2) Preparation of polyester elastomers containing olefins in side chains
[0042] 2.5 kg of dimethyl terephthalate, 0.5 kg of dimethyl isophthalate, 0.52 kg of dimethyl allyl malonate, 1.38 kg of 1,4-butanediol, 0.2 kg of ethylene glycol, and 2 kg of polyethylene glycol (M n =400g / mol), 2g of antimony trioxide, 0.8g of stannous octoate, 20g of antioxidant 1010 and 12g of antioxidant 168 were added into the reactor, and the temperature was raised to 190°C under nitrogen protection to carry out ester exchange reaction. After the reaction for 1h, the polymerization temperature was raised to 230°C, and polycondensation was carried out under a high vacuum of less than 100Pa for 6h to obtain a side chain olefin-containing polyester elastomer.
[0043] 3) Preparation of blood-compatible polyester elastomer
[0044] 1 kg of the side chain olefin-containing polyester elastomer was immersed in N-methylpyrrolidone containing 120 g of thiolated γ-polyglutamic acid and 33 g of benzophenone, then irradiated with an ultraviolet lamp (λ = 365 nm) for 4 h, washed with ethanol to remove the remaining reactants, and dried in an oven to obtain a blood-compatible polyester elastomer.
[0045] Example 3
[0046] The preparation method of the blood-compatible polyester elastomer of this embodiment comprises the following steps:
[0047] 1) Preparation of thiolated γ-polyglutamic acid
[0048] 20 g of γ-polyglutamic acid (molecular weight 100,000 Daltons) was dissolved in 4000 mL of MES buffer, and then 29.7 g of and 8.9 g of NHS, activated at room temperature for 90 min; then 12.2 g of L-cysteine hydrochloride dissolved in 1220 mL of MES buffer was added dropwise, 0.1 M HCl solution was added to adjust the pH value to 7, and then the reaction was protected from light under nitrogen at room temperature for 24 h, and then lyophilized after dialyzation to obtain a white powder, which is thiolated γ-polyglutamic acid.
[0049] 2) Preparation of polyester elastomers containing olefins in side chains
[0050] 3.5 kg of dimethyl terephthalate, 0.2 kg of dimethyl 2,6-naphthalene dicarboxylate, 0.2 kg of dimethyl allyl malonate, 2.2 kg of 1,4-butanediol, 0.7 kg of 1,3-propylene glycol, 2.5 kg of polyethylene glycol (M n=6000g / mol), 5g of ethylene glycol antimony, 1g of zinc acetate and 30g of antioxidant 1330 were added into the reactor, and the temperature was raised to 210°C under nitrogen protection to carry out ester exchange reaction. After the reaction for 0.5h, the polymerization temperature was raised to 250°C, and polycondensation was carried out under a high vacuum of less than 100Pa for 2h to obtain a side chain olefin-containing polyester elastomer.
[0051] 3) Preparation of blood-compatible polyester elastomer
[0052] 1 kg of the side chain olefin-containing polyester elastomer was immersed in an acetonitrile solution containing 33 g of thiolated γ-polyglutamic acid and 5.5 g of 2-hydroxy-2-methyl-1-phenyl-1-propanone, and then irradiated with an ultraviolet lamp (λ = 365 nm) for 0.1 h, washed with ethanol to remove the remaining reactants, and dried in an oven to obtain a blood-compatible polyester elastomer.
[0053] Example 4
[0054] The preparation method of the blood-compatible polyester elastomer of this embodiment comprises the following steps:
[0055] 1) Preparation of thiolated γ-polyglutamic acid
[0056] Thiolated γ-polyglutamic acid was prepared according to step 1) in Example 1.
[0057] 2) Preparation of polyester elastomers containing olefins in side chains
[0058] 6 kg of dimethyl terephthalate, 0.5 kg of dimethyl biphenyl dicarboxylate, 0.5 kg of dimethyl allyl malonate, 3.3 kg of ethylene glycol, 1.65 kg of polyethylene glycol (Mn=2000 g / mol), 1.2 g of dibutyl tin oxide and 12 g of antioxidant 1076 were added into the reactor. The temperature was raised to 185°C under nitrogen protection to carry out ester exchange reaction. After 1 hour of reaction, the polymerization temperature was raised to 240°C, and polycondensation was carried out under a high vacuum of less than 100 Pa for 3 hours to obtain a side chain olefin-containing polyester elastomer.
[0059] 3) Preparation of blood-compatible polyester elastomer
[0060] 1 kg of the side chain olefin-containing polyester elastomer was immersed in a tetrahydrofuran solution containing 64 g of thiolated γ-polyglutamic acid and 7 g of phenyl(2,4,6-trimethylbenzoyl)phosphate lithium salt, then irradiated with an ultraviolet lamp (λ=365 nm) for 4 h, washed with ethanol to remove the remaining reactants, and dried in an oven to obtain a blood-compatible polyester elastomer.
[0061] Example 5
[0062] The preparation method of the blood-compatible polyester elastomer of this embodiment comprises the following steps:
[0063] 1) Preparation of thiolated γ-polyglutamic acid
[0064] Thiolated γ-polyglutamic acid was prepared according to step 1) in Example 1.
[0065] 2) Preparation of polyester elastomers containing olefins in side chains
[0066] 2 kg of dimethyl terephthalate, 0.4 kg of dimethyl phthalate, 0.3 kg of dimethyl allyl malonate, 1.7 kg of 1,4-butanediol, 9.6 kg of polyethylene glycol (Mn=1000 g / mol), 8 g of tetraisopropyl titanate, 7 g of zinc acetate, 100 g of antioxidant 1330 and 40 g of antioxidant 168 were added into a reactor, and the temperature was raised to 190°C under nitrogen protection to carry out ester exchange reaction. After 1 hour of reaction, the polymerization temperature was raised to 260°C, and polycondensation was carried out under a high vacuum of less than 100 Pa for 5 hours to obtain a side chain olefin-containing polyester elastomer.
[0067] 3) Preparation of blood-compatible polyester elastomer
[0068] 1 kg of the side chain olefin-containing polyester elastomer was immersed in an N,N-dimethylformamide solution containing 80 g of thiolated γ-polyglutamic acid and 7 g of ethyl 4-dimethylaminobenzoate, then irradiated with an ultraviolet lamp (λ = 365 nm) for 0.1 h, washed with ethanol to remove the remaining reactants, and dried in an oven to obtain a blood-compatible polyester elastomer.
[0069] Comparative Example 1
[0070] The preparation method of the polyester elastomer of Comparative Example 1 is as follows: 3.3 kg of dimethyl terephthalate, 1.9 kg of 1,4-butanediol, and 2 kg of polyethylene glycol (M n =2000g / mol), 2.4g of tetrabutyl titanate, 2g of magnesium acetate and 16g of antioxidant 1098 were added into the reactor, and the temperature was raised to 180°C under nitrogen protection to carry out ester exchange reaction. After the reaction for 2h, the polymerization temperature was raised to 240°C, and polycondensation was carried out under a high vacuum of less than 100Pa for 4h to obtain a polyester elastomer.
[0071] Comparative Example 2
[0072] The preparation method of the polyester elastomer of Comparative Example 2 comprises the following steps:
[0073] 1) Preparation of thiolated γ-polyglutamic acid
[0074] Thiolated γ-polyglutamic acid was prepared according to step 1) in Example 1.
[0075] 2) Preparation of polyester elastomers containing olefins in side chains
[0076] 3 kg of dimethyl terephthalate, 0.9 kg of dimethyl allylmalonate, 1.9 kg of 1,4-butanediol, and 2 kg of polyethylene glycol (M n =2000g / mol), 2.4g of tetrabutyl titanate, 2g of magnesium acetate and 16g of antioxidant 1098 were added into the reactor, and the temperature was raised to 180°C under nitrogen protection to carry out ester exchange reaction. After 2h of reaction, the polymerization temperature was raised to 240°C, and polycondensed under a high vacuum of less than 100Pa for 4h to obtain a side chain olefin-containing polyester elastomer.
[0077] 3) Preparation of blood-compatible polyester elastomer
[0078] 1 kg of the side chain olefin-containing polyester elastomer was immersed in a dimethyl sulfoxide solution containing 210 g of thiolated γ-polyglutamic acid and 10 g of benzoin dimethyl ether, then irradiated with an ultraviolet lamp (λ = 365 nm) for 0.3 h, washed with ethanol to remove the remaining reactants, and dried in an oven to obtain a blood-compatible polyester elastomer.
[0079] Comparative Example 3
[0080] The difference from Example 1 is that polytetrahydrofuran ether glycol is used to replace the polyethylene glycol in Example 1 in an equal amount.
[0081] Comparative Example 4
[0082] The preparation method of the polyester elastomer of Comparative Example 4 is as follows: 1 kg of the polyester elastomer prepared in Comparative Example 1 is dissolved in 1500 mL of THF / MES buffer (the volume ratio of THF to MES is 4:1); 90 g of heparin sodium is dissolved in 1000 mL of THF / MES buffer (the volume ratio of THF to MES is 4:1), and 8 g of and 9 g of NHS, activated in an ice water bath for 1 h, then slowly dropwise added with THF / MES buffer containing polyester elastomer, reacted under nitrogen protection and light protection for 24 h at room temperature, dialyzed and freeze-dried to obtain heparinized polyester elastomer.
[0083] The polyester elastomers prepared in Examples 1-5 and Comparative Examples 1-4 were subjected to performance tests, and the test results are shown in Table 1:
[0084] Table 1 Performance test results of polyester elastomers of Examples 1-5 and Comparative Examples 1-4
[0085]
[0086] As can be seen from Table 1, the hardness of the polyester elastomer prepared in Examples 1-5 of the present invention is 25-74D, the calcium recovery time is 659-831min, the hemolysis rate is 0.15-0.45%, and the antibacterial rate is 97.3-99.4%. Therefore, after the introduction of γ-polyglutamic acid into the polyester elastomer of the present invention, the polyester elastomer exhibits excellent anticoagulant performance, low hemolytic toxicity and high antibacterial rate. The polyester elastomer prepared in Examples 4-5 has a significant difference in hardness from the polyester elastomer prepared in Examples 1-3 due to the different soft and hard segment contents, but it is these differences that enable polyester elastomers of different hardness to meet the needs of different fields, further expanding the application range of polyester elastomer materials.
[0087] By comparing Example 1 and Comparative Example 1, it is found that the anticoagulation ability of the polyester elastomer is greatly increased by the introduction of γ-polyglutamic acid, and the recalcification time is increased from 324min to 725min. This may be because the electrostatic effect and hydration layer formation ability of γ-polyglutamic acid can form a stable, dense and negatively charged hydration layer on the surface of the material. This hydration layer can prevent the aggregation and adhesion of red blood cells and platelets in the blood on the surface of the material, thereby prolonging the anticoagulation time of the material and reducing hemolytic toxicity. Compared with Comparative Example 1, Example 1 has enhanced antibacterial properties, which may be due to the fact that γ-polyglutamic acid contains amino groups, which will interact electrostatically with the cell membrane on the bacteria, thereby inhibiting or killing the bacteria. Compared with Comparative Example 2, the hardness of the polyester elastomer in Example 1 is reduced from 56D to 43D, which shows that the amount of γ-polyglutamic acid introduced into the polyester elastomer should not be too much, and too much will hinder the crystallization of the polyester elastomer and destroy the physical and mechanical properties of the polyester elastomer. Compared with Comparative Example 3, Example 1 shows that the recalcification time of the polyester elastomer is greatly increased and the hemolytic toxicity is greatly reduced, which may be caused by the superior hydrophilicity of polyethylene glycol to polytetrahydrofuran ether glycol. Compared with Comparative Example 4, Example 1 shows that the anticoagulant property of the polyester elastomer introduced with γ-polyglutamic acid is better than that of the heparinized polyester elastomer, and the recalcification time is 725min and 565min respectively, and the antibacterial property is also relatively excellent, which proves that the blood compatibility of the polyester elastomer after the introduction of γ-polyglutamic acid is better than that of the conventional anticoagulant heparin.
[0088] In summary, the present invention introduces γ-polyglutamic acid into the side chain of polyester elastomer to make the polyester elastomer have good blood compatibility, solve the problem of easy migration of anticoagulants and poor compatibility, and further expand the application range of polyester elastomer.
Claims
1. A method for preparing a blood-compatible polyester elastomer, characterized in that: The following steps are involved: S1 uses aromatic dibasic acid dimethyl ester, allyl dimethyl malonate, aliphatic diol and polyethylene glycol as raw materials, adds catalyst and antioxidant to carry out ester exchange reaction and polycondensation reaction to obtain side chain olefin-containing polyester elastomer; the molar ratio of aromatic dibasic acid dimethyl ester to aliphatic diol is 1: (1.2-1.8); allyl dimethyl malonate accounts for 5-15% of the total mass of dimethyl ester; the mass ratio of aromatic dibasic acid dimethyl ester to polyethylene glycol is (0.25-4): 1; S2 immerses the side chain olefin-containing polyester elastomer in an organic solvent containing thiolated γ-polyglutamic acid, and in the presence of a photoinitiator and under ultraviolet light irradiation, a thiol-ene click chemistry reaction occurs to prepare a blood-compatible polyester elastomer; the ratio of the mass percentage of thiolated γ-polyglutamic acid in the side chain olefin-containing polyester elastomer to the mass percentage of dimethyl allyl malonate in dimethyl ester is (1-1.5):
1.
2. The method for preparing a blood-compatible polyester elastomer according to claim 1, characterized in that: In step S1, the aromatic dibasic acid dimethyl ester is one or two of dimethyl terephthalate, dimethyl phthalate, dimethyl isophthalate, dimethyl biphenyl dicarboxylate and dimethyl 2,6-naphthalene dicarboxylate; the aliphatic diol is one or two of ethylene glycol, 1,3-propylene glycol and 1,4-butanediol.
3. The method for preparing a blood-compatible polyester elastomer according to claim 1, characterized in that: In step S1, the number average molecular weight of polyethylene glycol is 400-6000 g / mol.
4. The method for preparing a blood-compatible polyester elastomer according to claim 1, characterized in that: In step S1, the catalyst is one or two of zinc acetate, magnesium acetate, antimony trioxide, antimony glycol, dibutyltin oxide, stannous octoate, tetrabutyl titanate and tetraisopropyl titanate, and the added amount is 0.01-0.1% of the total mass of the raw materials.
5. The method for preparing a blood-compatible polyester elastomer according to claim 1, characterized in that: In step S1, the antioxidant is one or two of antioxidant 1010, antioxidant 1098, antioxidant 168, antioxidant 1076 and antioxidant 1330, and the added amount is 0.1-1% of the total mass of the raw materials.
6. The method for preparing a blood-compatible polyester elastomer according to claim 1, characterized in that: In step S1, the transesterification reaction temperature is 180-210°C, the reaction time is 0.5-2h; the polycondensation reaction temperature is 230-260°C, the reaction time is 2-6h, and the vacuum degree is <100Pa.
7. The method for preparing a blood-compatible polyester elastomer according to claim 1, characterized in that: In step S2, the preparation method of thiolated γ-polyglutamic acid is as follows: 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride and N-hydroxysuccinimide are added to a 2-(N-morpholino)ethanesulfonic acid buffer containing γ-polyglutamic acid, activated for 5-90 minutes, and then L-cysteine hydrochloride dissolved in the 2-(N-morpholino)ethanesulfonic acid buffer is added dropwise, and the pH value is adjusted to 4-7, and the reaction is carried out at room temperature with nitrogen protection to avoid light for 2-24 hours, and then lyophilized after dialysis to obtain a white powder, which is thiolated γ-polyglutamic acid.
8. The method for preparing a blood-compatible polyester elastomer according to claim 7, characterized in that: The molecular weight of γ-polyglutamic acid is 5000-100000 Daltons, the concentration of 2-(N-morpholino)ethanesulfonic acid buffer containing γ-polyglutamic acid is 5-20 g / L, the concentration of 2-(N-morpholino)ethanesulfonic acid buffer containing L-cysteine hydrochloride is 10-40 g / L, the molar ratio of 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride to N-hydroxysuccinimide is (1-2):1, and the molar ratio of carboxyl, 1-ethyl-(3-dimethylaminopropyl)carbodiimide hydrochloride to L-cysteine hydrochloride in γ-polyglutamic acid is 1:(1-2):(1-2).
9. The method for preparing a blood-compatible polyester elastomer according to claim 1, characterized in that: The photoinitiator is 2-hydroxy-2-methyl-1-phenylpropanone, benzoin dimethyl ether, benzophenone, phenyl (2,4,6-trimethylbenzoyl) phosphate lithium salt or 4-dimethylaminobenzoic acid ethyl ester, and the added amount is 0.5-3% of the total mass of the raw materials in step S2; the organic solvent is tetrahydrofuran, acetonitrile, N-methylpyrrolidone, dimethyl sulfoxide or N,N-dimethylformamide; the ultraviolet light irradiation time is 0.1-4h.
10. A blood-compatible polyester elastomer, characterized in that: The blood-compatible polyester elastomer is prepared by the preparation method of the blood-compatible polyester elastomer according to any one of claims 1 to 9.