12.9 grade annealing-free hot-rolled high carbon carbon cold heading steel wire rod and its manufacturing method
Through the chemical composition of hypoeutectoid high-carbon carbon with low hardenability and online molten salt pearlite temperature control technology, the microstructure of tempered pearlite and quasi-spheroidized alkalinity is formed, solving the problem of grade 12.9 fastener wire rod Eliminate cost and process complexity issues in anneal-free manufacturing, enabling efficient, green manufacturing of high-strength fasteners and reducing the risk of cracking.
Patent Information
- Application Number
- CN202410969479.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-19
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-07-19
AI Technical Summary
The existing hot-rolled cold-headed steel wire rods of grade 12.9 fasteners have problems such as high material cost, complex processes, high energy consumption and high risk of cracking during the annealing-free manufacturing process, making it difficult to meet the needs of high-strength and efficient green manufacturing.
Designed with hypoeutectoid high carbon chemical composition with low hardenability, including C: 0.65%~0.70%, Si: 0.15%~0.35%, Mn: 0.45%~0.55%, P≤0.0 15%, S≤0.015%, through online molten salt pearlite temperature control and roller slow cooling technology, the microstructure of tempered pearlite and quasi-spheroidized carbides is formed, reducing the formation of network carbides and improving the wire rod Strong plasticity.
It achieves annealing-free, efficient and green manufacturing of grade 12.9 high-strength fasteners, reduces the risk of cracking during drawing and cold heading processes, simplifies the manufacturing process, and improves the mechanical properties and production efficiency of the material.
Smart Images

Figure CN118497622B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of hot-rolled cold-heading steel wire rods, and in particular relates to a 12.9-grade annealing-free hot-rolled high-carbon carbon cold-heading steel wire rod and a manufacturing method thereof. Background Art
[0002] With the continuous development of the new energy vehicle field, the development of 12.9 grade ultra-high strength cold heading steel wire for fasteners requires the hot-rolled wire rod to be subjected to multiple spheroidizing annealing, drawing, cold heading, quenching and tempering processes in sequence to achieve the final performance level. The spheroidizing annealing process is to treat at 750~780℃ for 4~7h. The purpose is to soften the structure to improve the drawing and cold heading performance and reduce the risk of wire breakage and cold heading cracking of the wire rod. However, it also brings problems such as many processes, high manufacturing costs, high energy consumption and high emissions. Due to the annealing-free demand for green production of 12.9 ultra-high strength cold heading steel wire for fasteners, higher requirements are put forward for the design of raw material hot-rolled wire rod, especially the plasticity of the material.
[0003] The existing hot-rolled cold-heading steel wire rods used for simplifying annealing or even annealing-free manufacturing of 12.9 grade fasteners generally use medium and low carbon steel grades, and then add Cr, Mo, B, Ti and other alloy components to improve the hardenability or strength of the steel grades. After rolling and spinning, the wire rods with ferrite + pearlite microstructures are obtained under the Stelmor air cooling process to increase the proportion of ferrite in the structure to improve the plasticity of the wire rods. For example: CN117265408A discloses an annealing-free cold-heading steel and its manufacturing method and the fasteners obtained therefrom, which adopt a medium C-Si-Mn-Al-Cr-Mo-B-Mg composition design, combined with low temperature rolling The heat preservation and slow cooling process after wire drawing obtains a large part of ferrite + a small part of degraded pearlite structure, reaching Rm≤650MPa and area reduction rate ≥53%. However, on the one hand, the addition of multiple alloy components increases the material cost. In order to reduce the cost, reducing the alloy content or omitting the alloy will cause a significant decrease in the strength of the wire rod, making it difficult to reach the 12.9 performance level even after annealing. On the other hand, the addition of alloy components such as Cr, Ti, and B leads to high hardenability of the wire rod, and bainite, martensite and other brittle harmful structures that are not conducive to drawing are easily precipitated during the controlled cooling process after rolling. The risk of cracking increases during drawing and cold heading. At the same time, the design idea of increasing the proportion of ferrite in the organization to improve the plasticity of the wire rod will lead to a significant loss of wire rod strength. In the drawing process, a large reduction rate drawing is required to increase the strength of the wire rod and temper it to 12.9. The plasticity loss is large during the process, which also causes the risk of wire breakage or cracking. Therefore, some ultra-high strength fasteners use cold heading steel wire rods based on high hardenability components to retain a small amount of bainite in the organization to maintain the appropriate strength of the matrix. However, the dislocation density of bainite is high and the plastic hinge is poor, which is easy to cause wire breakage or cracking during wire rod coiling, transportation or downstream wire laying. It is easy to break, resulting in limited wire rod yield and narrow production window; although the patent CN118166189A discloses a 12.9 grade annealing-free hot-rolled complex phase cold heading steel wire rod and its manufacturing method, which adopts a medium C-Si-Mn-Cr composition design, combines molten salt ultra-fast cold quenching after spinning, online molten salt heating tempering and roller slow cooling to obtain a complex phase structure of tempered bainite, tempered martensite and quasi-spheroidized carbide, achieving a tensile strength of 1012~1063MPa and a cross-sectional shrinkage of 55%~59%, which can effectively improve the brittle phase problem, but requires two salt bath controls, and the process is not simplified enough.
[0004] Carbon is the most basic strengthening element in steel and is more economical than other elements. As the carbon content increases, the tensile strength of steel can be improved. Therefore, hot-rolled cold-heading steel wire rods made of high-carbon carbon steel without alloy components such as Cr, Ti, and B are used for annealing-free, efficient and green manufacturing of 12.9-grade fasteners, which is of great significance to reducing steel costs. However, the existing high-carbon hot-rolled wire rods are difficult to meet the technical difficulties and causes of annealing-free cold-heading manufacturing of 12.9-grade fasteners:
[0005] (1) With the increase of carbon content in steel, the segregation of molten steel during solidification increases. However, the length and maximum cooling capacity of the Stelmor air cooling line are limited. Low-carbon cold heading steel wire rods are more likely to precipitate secondary cementite, i.e., network carbide, along the grain boundaries during the Stelmor air cooling process after rolling due to the longer time spent in the secondary carbide precipitation zone. The presence of network carbides will weaken the connection between grains, increase the inhomogeneity of chemical composition in steel, reduce the utilization rate of carbon elements, and reduce the mechanical properties of steel, especially the sharp drop in plasticity and toughness. This will cause the material to break and crack due to uneven force or insufficient plasticity during annealing-free drawing or cold heading. In order to avoid the precipitation of network carbides when the wire-spinning temperature of high-carbon hot-rolled wire rods is low, or to reduce the wire-spinning temperature after wire-spinning, the wire rods will be more likely to break and crack due to uneven force or insufficient plasticity. Regarding the level of mesh carbon precipitated in the air-cooling section, the existing high-carbon hot-rolled wire rods will adopt medium-high temperature wire drawing and Stelmor rapid cooling processes. However, on the one hand, the rolling temperature and time of the wire rods under medium-high temperature wire drawing are relatively high, which can easily lead to coarse austenite grains, which is not conducive to maintaining the matrix strength and certain toughness of 12.9 grade cold heading steel wire rods for fasteners while reducing or eliminating alloy components. On the other hand, further improving the air cooling intensity will increase the difference in air volume between the windward side and the leeward side of the wire rod. The increased temperature difference of the wire rod will cause increased fluctuations in the mechanical properties of the wire rod, and also increase the risk of precipitation of abnormal bainite and martensite phases. At the same time, the incubation time of the wire rod after wire drawing is still relatively long after the diffusion-type mesh carbon. Although the amount of mesh carbon precipitation is reduced, the level is still relatively high, which in turn affects the wire rod production capacity and causes the risk of wire breakage or cracking in subsequent processing.
[0006] (2) The existing high-carbon hot-rolled wire rod for drawing processing mainly increases the cooling rate of the wire rod in the air cooling process after spinning to increase the degree of supercooling, promotes the phase transformation of the sorbite structure with a small interlamellar spacing, and increases the sorbite content in the structure and improves the sorbitization rate to improve the strength of the wire rod, so as to achieve the ultra-high strength of the product after drawing. However, the plasticity of the wire rod is lost to a certain extent. At the same time, with the increase of carbon content and the thickening of the structure lamellae, the spheroidization trend of carbides is slow. During the continuous cooling process, the wire rod passes through the sorbite phase transformation temperature range for a short time, resulting in high stress and dislocation density of the obtained hot-rolled wire rod structure. It cannot be softened at low temperature, and finally causes a large stress concentration in the matrix. The wire rod has insufficient plasticity, which makes it easy for carbides to break brittlely or form microcracks during drawing and cold heading. Reducing the cooling rate to increase the ferrite content in the structure will also lose the strength of the wire rod. The improvement of the plasticity of the wire rod is limited, and it is not conducive to improving the carbon mesh problem, and it is difficult to meet the annealing-free drawing and cold heading processing requirements of 12.9 grade fasteners. Summary of the invention
[0007] The present invention aims to solve at least one of the above-mentioned technical problems to a certain extent. The present invention provides a 12.9-grade annealing-free hot-rolled high-carbon carbon cold heading steel wire rod and a manufacturing method thereof, which can reduce material costs, simplify the manufacturing process, realize the microstructure regulation and strength-plasticity matching of the hot-rolled high-carbon carbon cold heading steel wire rod, and is used for the annealing-free, efficient and green manufacturing of 12.9-grade high-strength cold heading steel fasteners, which can reduce the risk of cracking during drawing and cold heading processing.
[0008] The technical solution adopted by the present invention to solve its technical problem is:
[0009] A 12.9 grade annealing-free hot-rolled high-carbon carbon cold heading steel wire rod, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.65%-0.70%, Si: 0.15%-0.35%, Mn: 0.45%-0.55%, P≤0.015%, S≤0.015%, and the rest is Fe and unavoidable impurities; its microstructure includes tempered pearlite accounting for 87%-92% by volume, and the rest is ferrite and quasi-spheroidized carbide.
[0010] The design basis of the chemical composition and mass percentage of the above-mentioned cold heading steel wire rod includes:
[0011] (1) Carbon: Carbon is the most basic and more economical strengthening element in steel than other elements. It exists in steel in the form of interstitial solid solution or carbide. Without adding Cr, Mo, B, Ti and other alloy components to improve the hardenability or strength of steel, as the carbon content increases, the tensile strength of steel can be significantly improved, but the plasticity and toughness decrease, increasing the risk of decarburization and the risk of cementite being distributed in a network along the pearlite grain boundary. At the same time, it makes the organizational layer thicker, affects the spheroidization trend of carbides, and further affects the content of quasi-spheroidized carbides produced when pearlite is softened at high temperature. Therefore, in order to enable the cold heading steel wire rod to achieve the final performance level of 12.9 grade fasteners through quenching and tempering under the annealing-free process, and at the same time reduce the difficulty of controlling network carbides and forming quasi-spheroidized carbides, taking into account the cold deformation performance of the cold heading steel wire rod, the mass percentage of C is controlled to be 0.65%~0.70%.
[0012] (2) Silicon: Si is a good deoxidizing element during steel smelting. It can also be dissolved in ferrite to improve the stability of supercooled austenite and the critical transformation temperature of steel in hypoeutectoid steel. However, excessive silicon will easily produce bainite structure due to the improvement of steel hardenability, reduce the plasticity and impact toughness of steel, and make cold heading more difficult. Therefore, the mass percentage of Si is controlled to be 0.15%~0.35%.
[0013] (3) Manganese: Mn is a good deoxidizer and desulfurizer in the steelmaking process. It exists in steel mainly in the form of substitutional solid solution, which can improve the strength and wear resistance of steel. However, too high Mn content will aggravate the segregation during the solidification process of the steel billet, resulting in poor uniformity of the steel. It is easy to produce bainite structure due to the improvement of the hardenability of the steel, and it affects the spheroidization of carbides due to the reduction of carbon activity. Therefore, the mass percentage of Mn is controlled to be 0.45%~0.55%.
[0014] (4) Phosphorus and sulfur: P and S are impurity elements. The lower the better. Therefore, P is controlled to be ≤ 0.015% and S is ≤ 0.015%.
[0015] Based on the above-mentioned design of low-cost, low-hardenability hypoeutectoid high-carbon carbon chemical composition of high C-Si-low Mn, the high-carbon carbon wire rod after hot rolling and controlled cooling abandons the traditional microstructure composed of troostite + ferrite. The cold heading steel wire rod microstructure contains most of the tempered pearlite and a small amount of inevitable ferrite structure. The tempered pearlite has the same strength characteristics as the pearlite, provides the matrix strength, and the high carbon component makes up for the strength loss when the alloy components such as Cr, Ti, and B are omitted. At the same time, the wire rod has low hardenability, which suppresses the nucleation rate of bainite or martensite in the wire rod during the cooling process after rolling. Pearlite has better plasticity and toughness than troostite with finer interlamellar spacing. The tempered pearlite obtained by high temperature softening can further eliminate the stress of the pearlite structure, reduce the dislocation density of the pearlite and the stress concentration of the matrix, so that the plasticity and toughness of the tempered pearlite are significantly improved compared with the pearlite structure, and the microstructure also contains a small amount of quasi-spheroidized carbides formed by the high temperature softening of the pearlite. The deformation hindering effect of the quasi-spheroidized carbides on the ferrite is significantly weakened. With the increase of the content of tempered pearlite and quasi-spheroidized carbides in the hypoeutectoid steel, the strength and plasticity of the cold heading steel wire rod are matched, especially compared with the existing high carbon carbon wire rod, the plasticity is significantly improved, and it can be used for the annealing-free, efficient and green manufacturing of 12.9 grade high-strength cold heading steel fasteners, reducing the risk of cracking during drawing and cold heading.
[0016] Preferably, the lamellar spacing of the tempered pearlite is 160~200nm, and the volume percentage of the ferrite is 6%~11%. The smaller the lamellar spacing of the tempered pearlite and the lower the ferrite content, the higher the strength of the cold heading steel wire rod and the lower the plasticity. The larger the lamellar spacing of the tempered pearlite and the higher the quasi-spheroidized carbide content, the lower the strength of the cold heading steel wire rod and the higher the plasticity. The lamellar spacing of the tempered pearlite and the proportion of ferrite and quasi-spheroidized carbides can be further controlled to further regulate the strength-plasticity matching of the cold heading steel wire rod.
[0017] Preferably, the network carbide of the cold heading steel wire rod is level 0. As the level of the network carbide decreases, the utilization rate of the C element in the steel and the uniformity of the chemical composition can be increased, the tissue stress can be further reduced, the mechanical properties of the steel can be improved, especially the impact resistance and plasticity can be improved, and the coarse network carbide can be prevented from causing the wire rod to crack during the drawing and cold heading process.
[0018] Preferably, the diameter of the cold heading steel wire rod is 14.0~22.0mm, the tensile strength Rm is 1110~1160MPa, and the cross-sectional shrinkage rate Z is 51%~56%. Compared with medium and low carbon cold heading steel wire rods, it has a certain tensile strength, and at the same time, compared with high carbon steel wire rods, it has significantly improved plasticity, which is manifested as a higher cross-sectional shrinkage rate. Therefore, the risk of wire breakage during drawing and cracking during cold heading can be reduced without annealing treatment, meeting the production application of 12.9 grade fasteners.
[0019] The use of the above-mentioned 12.9 grade annealing-free hot-rolled high-carbon carbon cold heading steel wire rod includes: being used to manufacture 12.9 grade fasteners through drawing, cold heading and tempering processes without the spheroidizing annealing process.
[0020] The manufacturing method of the above-mentioned 12.9 grade annealing-free hot-rolled high-carbon carbon cold heading steel wire rod comprises: rolling the production line wire according to the chemical composition of the 12.9 grade annealing-free hot-rolled high-carbon carbon cold heading steel wire rod, after the wire rod is spun into wire rod at a spinning temperature of ≥900°C, it is subjected to online molten salt pearlite temperature control treatment, so that the wire rod is cooled to the pearlite phase region at a cooling rate of ≥34°C / s for transformation, and at the same time, the pearlite formed by the isothermal promotion phase transformation undergoes high-temperature softening to form quasi-spheroidized carbides, and finally is slowly cooled by a roller to produce a cold heading steel wire rod whose microstructure includes 87% to 92% tempered pearlite by volume, and the rest is ferrite and quasi-spheroidized carbides.
[0021] The above-mentioned manufacturing method, based on the chemical composition of hypoeutectoid high carbon with low hardenability, avoids the formation of network carbides on the grain boundaries and austenitization of the structure at too low spinning temperature of the wire rod through appropriate spinning temperature. At the same time, after spinning, it is directly passed through a salt bath for online molten salt pearlite temperature control treatment. On the one hand, compared with air cooling, water cooling and other methods, it can not only utilize the rapid heat exchange capacity of molten salt, but also quickly cool the wire rod from the spinning temperature at an extremely fast cooling rate, which can skip the precipitation range of secondary cementite and quickly reach the high-temperature pearlite phase area, thereby preventing carbides from precipitating along the grain boundaries of austenite grains and avoiding the formation of network carbides on the hypoeutectoid high carbon carbon steel wire rod during the cooling process.
[0022] On the other hand, the wire rod can be fully in contact with the molten salt after passing through the molten salt to ensure uniform cooling. Compared with air cooling, there is no problem of temperature difference between the wind-exposed and wind-received surfaces of the wire rod, thereby uniform phase transformation occurs and the fluctuation of mechanical properties in the same circle is reduced. Combined with the low hardenability of the components, the precipitation of abnormal bainite and martensite phases can be avoided after temperature control. Compared with air cooling, after the wire rod temperature reaches the high-temperature pearlite phase region, it can maintain a long period of high-temperature isothermal state, which promotes the full incubation and transformation of the high-temperature austenite in the wire rod structure to the pearlite structure, forming a mixed structure composed mainly of pearlite and a small amount of ferrite structure, so as to ensure the strength and plasticity matching of the material. At the same time, due to the longer high-temperature isothermal effect rather than the slow air cooling line Continuous cooling can continuously soften the pearlite formed by high-temperature phase transformation during the temperature control process to form quasi-spheroidized carbides, eliminate tissue stress, and reduce tissue dislocation density, so as to further regulate the performance of the wire rod structure. At the same time, compared with two salt baths, this one salt bath can simplify the process, reduce the manufacturing difficulty, and improve the manufacturing efficiency. Finally, the high temperature state of the wire rod after passing through the molten salt can be utilized through roller slow cooling to further improve the softening effect of the wire rod in the process of dropping to the coiling temperature, so as to achieve the final organization, strength and plasticity regulation and economic production of the cold heading steel wire rod, and obtain a cold heading steel wire rod composed mainly of pearlite, a small amount of ferrite and quasi-spheroidized carbides.
[0023] Preferably, when heating the steel billet before rolling, the soaking temperature of the steel billet is controlled to be ≤1080°C, and the soaking time is ≤1.5h. High temperature can be used to promote uniform diffusion of components in the steel, while controlling low-temperature soaking to reduce the risk of decarburization, and avoid decarburization caused by excessively high soaking temperature and excessively long soaking time. Preferably, the soaking temperature is 1030~1080°C, the soaking time is 1~1.5h, and the total heating time is 4~5h.
[0024] Preferably, during the rolling, the initial rolling temperature is controlled to be 1020~1060℃, and the initial rolling deformation is 26%~34%. Since the online molten salt pearlite temperature control treatment stage can effectively improve the carbon mesh problem, the initial rolling temperature can be lower than the existing process, and the capacity of the rolling line in the rolling process can be reasonably utilized. The columnar crystals of the steel billet can be broken as much as possible with a lower initial rolling temperature and a larger initial rolling deformation, in preparation for grain refinement, and to avoid excessive initial rolling deformation, which makes it difficult to distribute a larger final rolling reduction.
[0025] Preferably, during the rolling, the final rolling temperature is controlled to be 930-975°C, and the final rolling reduction is 28-37%. On the basis of avoiding the subsequent spinning temperature being too low, as the final rolling temperature decreases and the final rolling reduction increases, the amount of deformed austenite recrystallization is increased, dynamic recrystallization occurs as much as possible, the grain size is reduced, and the grains of the wire rod after rolling are greatly refined. At the same time, compared with the strengthening effects such as solid solution, a certain plasticity will be lost. This fine grain strengthening can have a better strengthening and toughening effect on the final wire rod, and at the same time, the carbides precipitated along the grain boundaries are distributed on larger grain boundaries, which is beneficial to the improvement of the network carbides. The accumulated dislocation density structure can increase the nucleation rate, which is beneficial to the transformation of carbides to spheroidized structures during the subsequent online molten salt pearlite temperature control treatment.
[0026] Preferably, the spinning temperature is 900-945° C. Further controlling the spinning temperature can adapt to the temperature of the rolling process, while avoiding excessively high temperature causing grain coarsening and widmanstatten structure, creating conditions for pearlite phase deformation nuclei.
[0027] Preferably, during the online molten salt pearlite temperature control treatment, the temperature is controlled to be 570-620°C, and the treatment time is 500-750s. The higher the temperature control temperature, the larger the interlamellar spacing of the tempered pearlite, and the more proeutectoid ferrite, resulting in a decrease in the proportion of tempered pearlite in the organization, a decrease in the strength of the wire rod, and an increase in plasticity; the lower the temperature control temperature, the smaller the interlamellar spacing of the tempered pearlite, the smaller the proportion of ferrite in the organization, the increase in the strength of the wire rod, and the decrease in plasticity, but if the temperature control temperature is too low, bainite structure will appear, which significantly increases the brittleness of the wire rod; the treatment The longer the time, the better the high-temperature softening effect of pearlite, the higher the content of quasi-spheroidized carbides, the lower the strength of the wire rod and the higher the plasticity. However, if the processing time is too long, not only the energy consumption will increase and the production efficiency will decrease, but also the quasi-spheroidized carbides will grow together, resulting in a decrease in the strength and plasticity of the wire rod. The shorter the processing time, the higher the tissue stress and dislocation density, the lower the content of quasi-spheroidized carbides, the higher the strength of the wire rod and the lower the plasticity. Therefore, the temperature control temperature and processing time of the online molten salt pearlite temperature control treatment can be further adjusted to regulate the wire rod structure and strength and plasticity.
[0028] Preferably, since the cooling rate of the wire rod from the spinning temperature to the high-temperature pearlite phase region is relatively fast, during the online molten salt pearlite temperature control treatment, the molten salt circulation rate is controlled to be 480-680 t / h, and the molten salt temperature rise is ≤7°C. The molten salt temperature rise can be controlled by a larger molten salt circulation rate, thereby improving the temperature control accuracy and promoting uniform phase transformation of the wire rod structure.
[0029] Preferably, the roller speed of the wire rod passing through the molten salt is 18-30 m / min. At this roller speed, the processing time control of the wire rod and the temperature control temperature can be met, and the production rhythm can be further regulated.
[0030] Preferably, during the slow cooling by the roller, the wire rod is conveyed through the interior of the heat preservation cover at a roller speed of ≤0.6m / s, so that the wire rod is slowly cooled at a cooling rate of 0.55~0.85℃ / s until it is coiled. The roller speed and the wire rod cooling rate can be further controlled to extend the time that the wire rod is in a high temperature state, promote high temperature softening to form quasi-spheroidized carbides, and also avoid the cooling rate being too low to affect the production efficiency.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] (1) In view of the fact that the development of existing 12.9 ultra-high strength fastener cold heading steel wire rods puts forward higher requirements for the design of cold heading steel wire rods, alloy elements such as Cr, Ti, and B are usually added to low and medium carbon steels, which leads to improved hardenability of the wire rods and increased risk of cracking during drawing and cold heading processes. The hot-rolled cold heading steel wire rod of the present invention adopts a low hardenability hypoeutectoid high carbon chemical composition design, which can not only effectively reduce material costs, but also break the limitations on the application of hypoeutectoid high carbon steel grades in cold heading steel. Combined with the cold heading steel wire rods including The mixed structure of tempered pearlite as the main part and a small amount of ferrite and quasi-spheroidized carbide is controlled, so that the wire rod has a certain strength while significantly reducing the organizational stress and dislocation density and improving the plasticity of the wire rod. The cold heading steel wire rod product after hot rolling and cooling can reach a tensile strength of 1110~1160MPa, a cross-sectional shrinkage of 51%~56%, and a network carbide of grade 0. It is used in the manufacture of 12.9 grade annealing-free high-strength fasteners, bolts and other application fields, which can reduce the risk of cracking during drawing and cold heading processes and has good application prospects.
[0033] (2) The manufacturing method of the present invention controls the microstructure of the hot-rolled wire rod by designing a hypoeutectoid high-carbon carbon chemical composition with low hardenability, combining online molten salt pearlite temperature control and roller slow cooling technology. The hot-rolled wire rod is controlled to quickly skip the secondary cementite precipitation zone after hot rolling, which significantly improves the carbon network problem. Then, a long-term isothermal transformation is carried out in the high-temperature pearlite phase region to form a mixed structure composed of pearlite and ferrite. This not only ensures the strength and plasticity matching of the material, but also utilizes the pearlite formed by high-temperature phase transformation to continuously soften at high temperature during the temperature control process to form quasi-spheroidized carbides, and controls the microstructure of the hot-rolled wire rod to a tempered state without martensite and bainite structures. At the same time, only one molten salt treatment is required, which simplifies the manufacturing process. The 12.9 grade annealing-free hot-rolled high-carbon carbon cold heading steel wire rod is successfully prepared, which has good industrial adaptability.
[0034] (3) The manufacturing method of the present invention can improve the carbon content of the wire rod by online molten salt pearlite temperature control, while further controlling low-temperature heat-saturation and rolling, which can reduce the risk of decarburization, and make dynamic recrystallization and grain refinement as much as possible. The strength and plasticity of the wire rod can be improved by fine grain strengthening, and the softening effect of the wire rod can be further improved by slow cooling on a roller. The method is more suitable for drawing and cold heading processing, and has good industrial adaptability. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0036] Figure 1 is a metallographic structure diagram of Example 1 of the present invention;
[0037] Figure 2 is the metallographic structure diagram of Example 2 of the present invention;
[0038] Figure 3 is the metallographic structure diagram of Example 3 of the present invention;
[0039] Figure 4 It is the metallographic structure diagram of comparative example 6 of the present invention. DETAILED DESCRIPTION
[0040] The embodiments described below with reference to the accompanying drawings are exemplary and are only for illustration and do not limit the description of the features and characteristics of the present invention. They are intended to be used to explain the present invention and are sufficient to enable those skilled in the art to implement the present invention. They should not be construed as limiting the scope of the present invention, which is limited only by the appended claims. Embodiment 1:
[0041] A preferred embodiment of the manufacturing method of the 12.9 grade annealing-free hot-rolled high-carbon carbon cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.69%, Si: 0.26%, Mn: 0.45%, P: 0.015%, S: 0.013%, and the rest is Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of low temperature heating → low temperature rolling → spinning → online molten salt pearlite temperature control → roller slow cooling → coiling, specifically:
[0042] The low-temperature heating process is used to heat the steel billet with a specification of 220mm×220mm through a heating furnace to achieve a high-temperature steel billet that can be rolled into plastic. The heating furnace is heated in sequence according to the preheating section, the heating section and the soaking section. The risk of decarburization is reduced by low-temperature soaking. Specifically: the soaking temperature of the steel billet is controlled to be 1080°C, the soaking time is 1h, and the total heating time is 4h.
[0043] The low temperature rolling process is used to roll the steel billet coming out of the heating furnace into a wire with a diameter of 18 mm through a rolling line. The columnar crystals of the steel billet are broken as much as possible through low temperature initial rolling and a large initial rolling deformation to prepare for grain refinement. The dynamic recrystallization and grain refinement are carried out as much as possible through low temperature final rolling and a large final rolling reduction, which provides favorable conditions for the transformation of carbides into spheroidized structures, and avoids the risk of too low temperature causing the wire-spinning temperature to be too low and causing the risk of net carbon precipitation during wire-spinning. Specifically, the initial rolling temperature is controlled to be 1060°C, the initial rolling deformation is 32%, the final rolling temperature is 975°C, and the final rolling reduction is 31%.
[0044] The spinning process is used to turn the wire rod coming out of the rolling line into a wire rod through a spinning mechanism. The wire rod is spread on the roller and transported along the roller. Through an appropriate spinning temperature, it is avoided that the wire rod forms a network of carbides on the grain boundary and austenitizes the structure at an excessively low spinning temperature, and it is avoided that the grains are coarsened due to excessively high temperature, so as to create conditions for the deformation nucleus of the pearlite phase. Specifically, the spinning temperature is controlled to be 945°C.
[0045] The online molten salt pearlite temperature control adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by rollers and quickly cooled to the molten salt temperature for online molten salt pearlite temperature control treatment, so that the wire rod is cooled to the high-temperature pearlite phase region at a cooling rate of 36°C / s for transformation. Based on the high carbon component design, a mixed structure composed of pearlite and ferrite is formed to ensure the strong and plastic matching of the material. At the same time, the pearlite formed by the isothermal promotion phase transformation undergoes high-temperature softening to form quasi-spheroidized carbides to regulate the wire rod structure performance. Specifically: the temperature control temperature is 605°C, the processing time is 500s, the molten salt circulation volume is controlled to be 630t / h, the molten salt temperature rise is ≤7°C, and the roller speed of the wire rod passing through the molten salt is 30m / min.
[0046] The roller slow cooling process is to convey the wire rod coming out of the salt bath tank into the insulation cover by rollers for slow cooling treatment, so as to promote carbide spheroidization and further improve the softening effect of the wire rod. Specifically, the wire rod is conveyed through the insulation cover at a roller speed of 0.55m / s, so that the wire rod is slowly cooled to 365℃ at a cooling rate of 0.75℃ / s until it is coiled; the coiling process is used to coil the wire rod into a coil by a coiling drum, and the finished cold heading steel wire rod is obtained after packaging and storage. Its metallographic structure diagram is as follows Figure 1 shown.
[0047] Comparative Example 1:
[0048] A method for manufacturing hot-rolled high-carbon carbon steel wire rod, the manufacturing method differs from Example 1 in that: the manufacturing method is manufactured according to the process flow of heating → rolling → spinning → Stelmor rapid cooling → roller slow cooling → coiling, specifically: the steel billet uniform heating temperature of the heating process is 1110°C; the initial rolling temperature of the rolling process is 1100°C, the final rolling temperature is 1010°C, and the spinning process controls the spinning temperature to 980°C; the Stelmor rapid cooling adopts 1~6# fans to be turned on at 95%, so that the wire rod is cooled to 605°C at a cooling rate of 9.6°C / s, and the roller slow cooling adopts closing all fans and insulation covers, so that the wire rod completes phase change in the cover at a cooling rate of 1.5°C / s, and the finished wire rod is obtained after coiling off the line.
[0049] Comparative Example 2:
[0050] A method for manufacturing hot-rolled high-carbon carbon steel wire rod, the manufacturing method differs from Example 1 in that: the manufacturing method is manufactured according to the process flow of heating → rolling → spinning → Stelmor rapid cooling → roller slow cooling → coiling, specifically: the steel billet uniform heating temperature of the heating process is 995°C; the initial rolling temperature of the rolling process is 980°C, the final rolling temperature is 890°C, and the spinning process controls the spinning temperature to be 860°C; the Stelmor rapid cooling adopts 100% opening of 1~7# fans to cool the wire rod to 570°C at a cooling rate of 10.3°C / s, the roller slow cooling adopts closing of all fans and insulation covers to complete the phase change of the wire rod in the cover at a cooling rate of 1.2°C / s, and the finished wire rod is obtained after coiling off the line. Embodiment 2:
[0051] A preferred embodiment of the manufacturing method of the 12.9 grade annealing-free hot-rolled high-carbon carbon cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.65%, Si: 0.35%, Mn: 0.52%, P: 0.014%, S: 0.01%, and the rest is Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of low temperature heating → low temperature rolling → spinning → online molten salt pearlite temperature control → roller slow cooling → coiling, specifically:
[0052] The low-temperature heating process is used to heat the steel billet with a specification of 220mm×220mm through a heating furnace to achieve a high-temperature steel billet that can be rolled and plastic. The heating furnace is heated in sequence according to the preheating section, the heating section and the soaking section. The risk of decarburization is reduced by low-temperature soaking. Specifically: the soaking temperature of the steel billet is controlled to be 1040°C, the soaking time is 1.2h, and the total heating time is 4.5h.
[0053] The low temperature rolling process is used to roll the steel billet coming out of the heating furnace into a wire with a diameter of 14 mm through a rolling line. Through low temperature initial rolling and a large initial rolling deformation, the columnar crystals of the steel billet are broken as much as possible to prepare for grain refinement. Through low temperature final rolling and a large final rolling reduction, dynamic recrystallization and grain refinement are carried out as much as possible, providing favorable conditions for the transformation of carbides to spheroidized structures, while avoiding the risk of too low temperature causing the wire-spinning temperature to be too low and causing the risk of net carbon precipitation during wire-spinning. Specifically: the initial rolling temperature is controlled to be 1032°C, the initial rolling deformation is 34%, the final rolling temperature is 945°C, and the final rolling reduction is 37%.
[0054] The spinning process is used to turn the wire rod coming out of the rolling line into a wire rod through a spinning mechanism. The wire rod is spread on the roller and transported along the roller. Through an appropriate spinning temperature, it is avoided that the wire rod forms a network of carbides on the grain boundary and austenitizes the structure at an excessively low spinning temperature, and it is avoided that the grains are coarsened due to excessively high temperature, so as to create conditions for the deformation nucleus of the pearlite phase. Specifically, the spinning temperature is controlled to be 920°C.
[0055] The online molten salt pearlite temperature control adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by rollers and quickly cooled to the molten salt temperature for online molten salt pearlite temperature control treatment, so that the wire rod is cooled to the high-temperature pearlite phase region at a cooling rate of 37°C / s for transformation. Based on the high-carbon component design, a mixed structure composed of pearlite and ferrite is formed to ensure the strong and plastic matching of the material. At the same time, the pearlite formed by the isothermal promotion phase transformation undergoes high-temperature softening to form quasi-spheroidized carbides to regulate the wire rod structure performance. Specifically: the temperature control temperature is 570°C, the processing time is 559s, the molten salt circulation volume is controlled to be 680t / h, the molten salt temperature rise is ≤7°C, and the roller speed of the wire rod passing through the molten salt is 26m / min.
[0056] The roller slow cooling process is to convey the wire rod coming out of the salt bath tank into the insulation cover by rollers for slow cooling treatment, so as to promote carbide spheroidization and further improve the softening effect of the wire rod. Specifically, the wire rod is conveyed through the insulation cover at a roller speed of 0.45m / s, so that the wire rod is slowly cooled to 352℃ at a cooling rate of 0.55℃ / s until it is coiled; the coiling process is used to coil the wire rod into a coil by a coiling drum, and the finished cold heading steel wire rod is obtained after packaging and storage. Its metallographic structure diagram is as follows Figure 2 shown.
[0057] Comparative Example 3:
[0058] A method for manufacturing a hot-rolled high-carbon carbon steel wire rod, the manufacturing method of which differs from that of Example 2 in that: the soaking temperature is 1088°C, the initial rolling temperature is 1082°C, the initial rolling deformation is 39%, the final rolling temperature is 992°C, the final rolling reduction is 22%, the wire laying temperature is 960°C, and the finished wire rod is obtained after coiling and rolling off the line.
[0059] Comparative Example 4:
[0060] A method for manufacturing hot-rolled high-carbon carbon steel wire rod, the manufacturing method of which differs from that of Example 2 in that the wire rod is cooled at a cooling rate of 30°C / s in a salt bath, the temperature is controlled at 635°C, and the finished wire rod is obtained after being rolled off the production line.
[0061] Comparative Example 5:
[0062] A method for manufacturing hot-rolled high-carbon carbon steel wire rod, the manufacturing method of which differs from that of Example 2 in that the wire rod is cooled at a cooling rate of 36°C / s in a salt bath, the temperature is controlled at 560°C, and the finished wire rod is obtained after being rolled off the production line.
[0063] Comparative Example 6:
[0064] A method for manufacturing hot-rolled high-carbon carbon steel wire rod, the difference between the manufacturing method and Example 2 is that the wire rod is cooled at a cooling rate of 45°C / s in a salt bath, the temperature is controlled at 350°C, the molten salt circulation rate is 730t / h, and the finished wire rod is obtained after the coil is rolled off the line. Embodiment 3:
[0065] A preferred embodiment of the manufacturing method of the 12.9 grade annealing-free hot-rolled high-carbon carbon cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.68%, Si: 0.32%, Mn: 0.48%, P: 0.015%, S: 0.015%, and the rest is Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of low temperature heating → low temperature rolling → spinning → online molten salt pearlite temperature control → roller slow cooling → coiling, specifically:
[0066] The low-temperature heating process is used to heat the steel billet with a specification of 220mm×220mm through a heating furnace to achieve a high-temperature steel billet that can be rolled into plastic. The heating furnace is heated in sequence according to the preheating section, the heating section and the soaking section. The risk of decarburization is reduced by low-temperature soaking. Specifically: the soaking temperature of the steel billet is controlled to be 1030°C, the soaking time is 1.2h, and the total heating time is 4.5h.
[0067] The low temperature rolling process is used to roll the steel billet coming out of the heating furnace into a wire with a diameter of 20 mm through a rolling line. Through low temperature initial rolling and a large initial rolling deformation, the columnar crystals of the steel billet are broken as much as possible to prepare for grain refinement. Through low temperature final rolling and a large final rolling reduction, dynamic recrystallization and grain refinement are carried out as much as possible, providing favorable conditions for the transformation of carbides to spheroidized structures, while avoiding the risk of too low temperature causing the wire-spinning temperature to be too low and causing the risk of net carbon precipitation during wire-spinning. Specifically: the initial rolling temperature is controlled to be 1020°C, the initial rolling deformation is 28%, the final rolling temperature is controlled to be 930°C, and the final rolling reduction is controlled to be 35%.
[0068] The spinning process is used to turn the wire rod coming out of the rolling line into a wire rod through a spinning mechanism. The wire rod is spread on the roller and transported along the roller. Through an appropriate spinning temperature, it is avoided that the wire rod forms a network of carbides on the grain boundary and austenitizes the structure at an excessively low spinning temperature, and it is avoided that the grains are coarsened due to excessively high temperature, so as to create conditions for the deformation nucleus of the pearlite phase. Specifically, the spinning temperature is controlled to be 900°C.
[0069] The online molten salt pearlite temperature control adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by rollers and quickly cooled to the molten salt temperature for online molten salt pearlite temperature control treatment, so that the wire rod is cooled to the high-temperature pearlite phase region at a cooling rate of 34°C / s for transformation. Based on the high-carbon component design, a mixed structure composed of pearlite and ferrite is formed to ensure the strong and plastic matching of the material. At the same time, the pearlite formed by the isothermal promotion phase transformation undergoes high-temperature softening to form quasi-spheroidized carbides to regulate the wire rod structure performance. Specifically: the temperature control temperature is 587°C, the processing time is 750s, the molten salt circulation volume is controlled to be 480t / h, the molten salt temperature rise is ≤7°C, and the roller speed of the wire rod passing through the molten salt is 18m / min.
[0070] The roller slow cooling process is to convey the wire rod coming out of the salt bath tank into the insulation cover by rollers for slow cooling treatment, so as to promote carbide spheroidization and further improve the softening effect of the wire rod. Specifically, the wire rod is conveyed through the insulation cover at a roller speed of 0.5m / s, so that the wire rod is slowly cooled to 360°C at a cooling rate of 0.62°C / s until it is coiled; the coiling process is used to coil the wire rod into a coil by a coiling drum, and the finished cold heading steel wire rod is obtained after packaging and storage. Its metallographic structure diagram is as follows Figure 3 shown.
[0071] Comparative Example 7:
[0072] A method for manufacturing hot-rolled high-carbon carbon steel wire rod, the manufacturing method of which is different from that of Example 3 in that the processing time is 800s, the roller speed of the wire rod passing through the molten salt is 15m / min, and the finished wire rod is obtained after the coil is rolled off the line.
[0073] Comparative Example 8:
[0074] A method for manufacturing hot-rolled high-carbon carbon steel wire rod, the manufacturing method of which is different from that of Example 3 in that the processing time is 910s, the roller speed of the wire rod passing through the molten salt is 13m / min, and the finished wire rod is obtained after the coil is rolled off the line.
[0075] Comparative Example 9:
[0076] A method for manufacturing hot-rolled high-carbon carbon steel wire rod, the manufacturing method of which is different from that of Example 3 in that the processing time is 458s, the roller speed of the wire rod passing through the molten salt is 30m / min, and the finished wire rod is obtained after the coil is rolled off the line. Embodiment 4:
[0077] A preferred embodiment of the manufacturing method of the 12.9 grade annealing-free hot-rolled high-carbon carbon cold heading steel wire rod of the present invention, the chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.7%, Si: 0.15%, Mn: 0.55%, P: 0.014%, S: 0.013%, and the rest is Fe and unavoidable impurities; the manufacturing method is manufactured according to the process flow of low temperature heating → low temperature rolling → spinning → online molten salt pearlite temperature control → roller slow cooling → coiling, specifically:
[0078] The low-temperature heating process is used to heat the steel billet with a specification of 220mm×220mm through a heating furnace to achieve a high-temperature steel billet that can be rolled and plastic. The heating furnace is heated in sequence according to the preheating section, the heating section and the soaking section. The risk of decarburization is reduced by low-temperature soaking. Specifically: the soaking temperature of the steel billet is controlled to be 1050°C, the soaking time is 1.5h, and the total heating time is 5h.
[0079] The low temperature rolling process is used to roll the steel billet coming out of the heating furnace into a wire with a diameter of 22 mm through a rolling line. Through low temperature initial rolling and a large initial rolling deformation, the columnar crystals of the steel billet are broken as much as possible to prepare for grain refinement. Through low temperature final rolling and a large final rolling reduction, dynamic recrystallization and grain refinement are carried out as much as possible, providing favorable conditions for the transformation of carbides to spheroidized structures, while avoiding the risk of too low temperature causing the wire-spinning temperature to be too low and causing the risk of net carbon precipitation during wire-spinning. Specifically: the initial rolling temperature is controlled to be 1045°C, the initial rolling deformation is 26%, the final rolling temperature is controlled to be 965°C, and the final rolling reduction is controlled to be 28%.
[0080] The spinning process is used to turn the wire rod coming out of the rolling line into a wire rod through a spinning mechanism. The wire rod is spread on the roller and transported along the roller. Through an appropriate spinning temperature, it is avoided that the wire rod forms a network of carbides on the grain boundary and austenitizes the structure at an excessively low spinning temperature, and it is avoided that the grains are coarsened due to excessively high temperature, so as to create conditions for the deformation nucleus of the pearlite phase. Specifically, the spinning temperature is controlled to be 938°C.
[0081] The online molten salt pearlite temperature control adopts a salt bath tank with molten salt inside. The wire rod after spinning is conveyed through the salt bath tank by rollers and quickly cooled to the molten salt temperature for online molten salt pearlite temperature control treatment, so that the wire rod is cooled to the high-temperature pearlite phase region at a cooling rate of 35°C / s for transformation. Based on the high-carbon component design, a mixed structure composed of pearlite and ferrite is formed to ensure the strong and plastic matching of the material. At the same time, the pearlite formed by the isothermal promotion phase transformation undergoes high-temperature softening to form quasi-spheroidized carbides to regulate the wire rod structure properties. Specifically: the temperature control temperature is 620°C, the processing time is 625s, the molten salt circulation volume is controlled to be 520t / h, the molten salt temperature rise is ≤7°C, and the roller speed of the wire rod passing through the molten salt is 22m / min.
[0082] The roller slow cooling process uses rollers to convey the wire rods coming out of the salt bath tank into the insulation cover for slow cooling treatment, which promotes carbide spheroidization and further improves the softening effect of the wire rod. Specifically: the wire rods are conveyed through the insulation cover at a roller speed of 0.6m / s, so that the wire rods are slowly cooled to 371°C at a cooling rate of 0.8°C / s until they are coiled; the coiling process is used to coil the wire rods into coils through a coiling drum, and the finished cold heading steel wire rods are obtained after packaging and storage.
[0083] Comparative Example 10:
[0084] A method for manufacturing a hot-rolled high-carbon carbon steel wire rod, the difference between the manufacturing method and Example 4 is that: the manufacturing method is manufactured according to the process flow of low-temperature heating → low-temperature rolling → spinning → online molten salt pearlite temperature control → air cooling → coiling, specifically: the air cooling process adopts the method of opening the insulation cover, and conveying the wire rod coming out of the salt bath tank by a roller at a roller speed of 0.85m / s, so that the wire rod is cooled at a cooling rate of 2.2℃ / s until it is coiled, and the finished wire rod is obtained after the coiling is off the line.
[0085] The wire rods obtained in the above embodiments and comparative examples were subjected to organizational and performance tests: the tensile test was conducted using "GB-T 228.1-2021 Metallic Material Tensile Test Part 1: Room Temperature Test Method" to obtain tensile strength and cross-sectional shrinkage, and the organizational test was conducted according to the metal microstructure test method of GB / T13298 standard. The comparative results obtained are shown in Table 1 below:
[0086] Table 1. Comparison of the microstructure and properties of cold heading steel wire rods with different compositions and manufacturing methods
[0087]
[0088] From the comparison results of Example 1 and Comparative Example 1, it can be seen that compared with the pearlite and ferrite structures obtained by the high-temperature spinning and air-cooling rapid cooling process, there are also higher levels of network carbide defects. The present invention uses a hypoeutectoid high-carbon carbon chemical composition design with low hardenability, combined with online molten salt pearlite temperature control and roller slow cooling technology, to control the hot-rolled wire rod structure, and by controlling the wire rod after hot-rolled spinning to undergo ultra-rapid cooling through online molten salt pearlite temperature control, the secondary cementite precipitation interval is quickly skipped, which significantly improves the network carbon problem, and the network carbide can reach level 0. At the same time, from the comparison results of Example 1 with Comparative Examples 1 and Comparative Examples 2, it can be seen that compared with the troostite and ferrite structures obtained by the low-temperature spinning and air-cooling rapid cooling process, there are also higher levels of network carbide defects. On the basis of effectively improving the carbon mesh problem, the present invention also utilizes a direct salt bath after spinning to perform a long-term isothermal transformation in the high-temperature pearlite phase region to form a mixed structure composed of most pearlite and a small amount of ferrite. The pearlite formed by the high-temperature phase transformation is continuously softened at high temperature during the temperature control process to form quasi-spheroidized carbides, and the hot-rolled wire rod structure is regulated to a tempered state, which can significantly reduce the structural stress and dislocation density, improve the wire rod plasticity, and the cold-headed steel wire rod product after hot rolling and cooling can reach a tensile strength of 1110~1160MPa and a cross-sectional shrinkage rate of 51~56%. It is used in the manufacture of 12.9-grade annealing-free high-strength fasteners and bolts and other application fields, can reduce the risk of cracking during drawing and cold heading processing, and has good application prospects.
[0089] From the comparison results of Example 2 and Comparative Example 3, it can be seen that compared with high-temperature soaking and rolling, the grains will be coarsened after rolling, and it is not conducive to the transformation of carbides to spheroidized structures during the subsequent online molten salt pearlite temperature control treatment. Further control of low-temperature soaking and rolling can reduce the risk of decarburization, and dynamically recrystallize and refine the grains as much as possible, and use fine grain strengthening to improve the plasticity and toughness of the wire rod.
[0090] From the comparison results of Examples 1 to 4 and Comparative Example 4, it can be seen that the higher the temperature control temperature, the larger the spacing between the tempered pearlite lamellae, the more proeutectoid ferrite, resulting in a decrease in the proportion of tempered pearlite in the organization, a decrease in the strength of the wire rod, and an increase in plasticity, but excessive temperature control temperature will cause a large loss in the strength of the cold heading steel wire rod; from the comparison results of Examples 1 to 4 and Comparative Example 5, it can be seen that the lower the temperature control temperature, the smaller the spacing between the tempered pearlite lamellae, the smaller the proportion of ferrite in the organization, the increase in the strength of the wire rod and the decrease in plasticity, but too low temperature control temperature will cause a large loss in the plasticity of the cold heading steel wire rod; and from the results of Comparative Example 6, it can be seen that if the temperature control temperature is too low, bainite structure will appear, which will significantly increase the brittleness of the wire rod.
[0091] From the comparison results of Examples 1 to 4 and Comparative Example 7, it can be seen that the longer the treatment time, the better the high-temperature softening effect of pearlite, the more quasi-spheroidized carbide content, the lower the wire rod strength and the higher the plasticity, but too long a treatment time will lead to a large loss of strength of the cold heading steel wire rod; from the comparison results of Examples 1 to 4 and Comparative Example 8, it can be seen that further increase in the treatment time will also cause the quasi-spheroidized carbides to grow together, resulting in a decrease in both the strength and plasticity of the wire rod; from the comparison results of Examples 1 to 4 and Comparative Example 9, it can be seen that the shorter the treatment time, the higher the tissue stress and dislocation density, the lower the quasi-spheroidized carbide content, the higher the wire rod strength and the lower the plasticity, so the temperature control temperature and treatment time of the online molten salt pearlite temperature control treatment can be further adjusted to regulate the wire rod structure and strength-plastic properties.
[0092] From the comparison results of Examples 1 to 4 and Comparative Example 10, it can be seen that compared with the weakened softening effect after air cooling, roller slow cooling is further adopted after the online molten salt pearlite temperature control treatment, and the roller speed and the wire rod cooling speed are controlled to extend the time that the wire rod is in a high temperature state, which can continue to promote high-temperature softening to form quasi-spheroidized carbides, and has good industrial adaptability.
[0093] The series of detailed descriptions listed above are only specific descriptions of feasible embodiments of the present invention. They are not intended to limit the scope of protection of the present invention. All equivalent embodiments or changes that do not deviate from the technical spirit of the present invention should be included in the scope of protection of the present invention.
Claims
1. A 12.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod, characterized in that: The chemical composition and mass percentage of the cold heading steel wire rod include: C: 0.65% to 0.70%, Si: 0.15% to 0.35%, Mn: 0.45% to 0.55%, P≤0.015%, S≤0.015%, and the remainder is Fe and unavoidable impurities; its microstructure includes tempered pearlite accounting for 87% to 92% by volume, and the remainder is ferrite and quasi-spheroidized carbides; The manufacturing method includes: rolling the wire rod according to the chemical composition of the 12.9 grade annealing-free hot-rolled high-carbon carbon cold heading steel wire rod, spinning the wire rod into a wire rod at a spinning temperature of 900-945°C, and then subjecting the wire rod to online molten salt pearlite temperature control treatment, so that the wire rod is cooled to the pearlite phase region at a cooling rate of ≥34°C / s for transformation, and at the same time, the pearlite formed by the phase transformation is isothermally promoted to undergo high-temperature softening to form quasi-spheroidized carbides, and finally, it is subjected to roller slow cooling to produce a cold heading steel wire rod with a microstructure including tempered pearlite, ferrite and quasi-spheroidized carbides; during the online molten salt pearlite temperature control treatment, the temperature is controlled to be 570-620°C, and the treatment time is 500-750s. During the roller slow cooling, the wire rod is conveyed through the inside of the heat preservation cover at a roller speed of ≤0.6m / s, so that the wire rod is slowly cooled at a cooling rate of 0.55-0.85°C / s until it is coiled.
2. The 12.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod according to claim 1, characterized in that: The interlamellar spacing of the tempered pearlite is 160-200 nm, the volume percentage of the ferrite is 6%-11%, and the network carbide of the cold heading steel wire rod is level 0.
3. The 12.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod according to claim 1, characterized in that: The cold heading steel wire rod has a diameter of 14.0-22.0 mm, a tensile strength of 1110-1160 MPa, and a cross-sectional shrinkage rate of 51%-56%.
4. A method for manufacturing 12.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod, characterized in that: The manufacturing method comprises: rolling the wire rod according to the chemical composition of the 12.9 grade annealing-free hot-rolled high carbon carbon cold heading steel wire rod as claimed in claim 1, spinning the wire rod into a wire rod at a spinning temperature of 900-945°C, and then subjecting the wire rod to an online molten salt pearlite temperature control treatment, so that the wire rod is cooled at a cooling rate of ≥34°C / s to the pearlite phase region for transformation, while isothermally promoting the pearlite formed by phase transformation to undergo high temperature softening to form quasi-spheroidized carbides, and finally slowly cooling the wire rod through a roller to produce the wire rod. The microstructure includes 87% to 92% by volume of tempered pearlite, and the rest is ferrite and quasi-spheroidized carbide of the cold heading steel wire rod. During the online molten salt pearlite temperature control treatment, the temperature is controlled at 570 to 620°C and the treatment time is 500 to 750s. During the roller slow cooling, the wire rod is conveyed through the inside of the insulation cover at a roller speed of ≤0.6m / s, so that the wire rod is slowly cooled at a cooling rate of 0.55 to 0.85°C / s until it is coiled.
5. The method for manufacturing 12.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod according to claim 4, characterized in that: When heating the steel billet before rolling, the steel billet soaking temperature is controlled to be ≤1080°C and the soaking time is controlled to be ≤1.5h.
6. The method for manufacturing 12.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod according to claim 4, characterized in that: During the rolling, the initial rolling temperature is controlled to be 1020-1060° C., and the initial rolling deformation is 26%-34%.
7. The method for manufacturing 12.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod according to claim 6, characterized in that: During the rolling, the final rolling temperature is controlled to be 930-975° C., and the final rolling reduction is controlled to be 28-37%.
8. The method for manufacturing 12.9 grade annealing-free hot-rolled high carbon cold heading steel wire rod according to claim 4, characterized in that: During the online molten salt pearlite temperature control treatment, the molten salt circulation rate is controlled to be 480-680 t / h, the molten salt temperature rise is ≤7°C, and the roller speed of the wire rod passing through the molten salt is 18-30 m / min.