A multilayer imide sintered winding round wire for submersible motor and a manufacturing method thereof
Through the production method of multi-layer imide sintered winding round wire, the combination of insulation modified paint and polyimide film layer is used to solve the problem of poor insulation performance and wear resistance of sintered winding round wire, and significantly improve the insulation of the product. and acid corrosion resistance.
Patent Information
- Application Number
- CN202410948078.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2044-07-16
AI Technical Summary
The existing sintered winding round wire has poor insulation performance and wear resistance, making it difficult to meet the requirements of special motor units. In particular, its stability is insufficient under acid corrosion conditions, which limits the efficiency of the product.
The production method of multi-layer imide sintered winding round wire is adopted, including the infiltration treatment of insulation modified paint, sintering of polyimide film and curing of immersion agent, using raw materials such as silicone resin, m-phenylenediamine, nano-mica agent, etc., together with the blending process. Effective agent and modified nano-silica agent to form a multi-layer structure to improve insulation and wear resistance.
The insulation, wear resistance and acid corrosion resistance stability of the product have been significantly optimized, and the synergistic improvement of insulation and wear resistance has been coordinated through multi-layer improved structure and material deployment.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of round wires, and in particular to a multi-layer imide sintered winding round wire for a submersible motor and a manufacturing method thereof. Background Art
[0002] Ordinary sintered enameled winding wires include enameled winding wires, glass fiber wrapped winding wires and paper wrapped winding wires. Generally, insulating varnish is applied to the conductor surface by dipping and baking, or glass fiber or insulating paper is wrapped on the conductor surface by wrapping. Since there is no strong bonding force between the conductor and the insulating layer, these products can usually only be used to wind conventional transformers, reactors and motor coils. Ordinary sintered enameled winding wires cannot meet the requirements of special motor groups for coils.
[0003] The existing sintered winding round wire has poor insulation performance and poor wear resistance. It is difficult to improve the insulation and wear resistance of the product in a coordinated manner, which limits the use efficiency of the product. In addition, the product has poor stability under acid corrosion conditions, which further limits the use efficiency of the product. Summary of the invention
[0004] In view of the defects of the prior art, the purpose of the present invention is to provide a multi-layer imide sintered winding round wire for a submersible motor and a manufacturing method thereof, so as to solve the problems raised in the above background technology.
[0005] The present invention solves the technical problem by adopting the following technical solution:
[0006] The present invention provides a multi-layer imide sintered winding round wire for a submersible motor. The sintered winding round wire comprises a round wire substrate. The round wire substrate is firstly treated by infiltration with an insulating modified paint to form an insulating paint layer. A polyimide film is then wound around the insulating paint layer and sintered to form a polyimide film layer. Finally, an impregnating agent is used for coating and then cured to form a modified layer. Thus, the multi-layer imide sintered winding round wire can be obtained.
[0007] The insulating modified paint comprises the following raw materials in parts by weight:
[0008] 25-30 parts of organic silicon resin, 2-5 parts of m-phenylenediamine, 5-8 parts of conditioning agent, 20-25 parts of xylene, and 4-7 parts of nano-mica agent; the preparation method of the conditioning agent is as follows:
[0009] S1: immersing the glass fiber into a sufficient amount of sodium silicate solution for immersion treatment, and then filtering and drying to obtain an immersed glass fiber agent;
[0010] S2: 2-5 parts of modified nano-silica agent, 3-5 parts of sodium lignin sulfonate solution, 1-3 parts of silane coupling agent KH560 and 4-7 parts of 5% by mass lanthanum nitrate solution are fully mixed to obtain a nano-silica conditioning solution;
[0011] S3: The immersed glass fiber agent and nano-silicon dioxide conditioning solution are mixed in a weight ratio of 5:3 and ball-milled at a ball-milling speed of 1000-1500 r / min for 2 hours. After the ball-milling is completed, the mixture is washed with water and dried to obtain a conditioning agent.
[0012] Preferably, the sintering process temperature is 200-230° C., and the sintering time is 2-5 min; the curing temperature is 155-165° C., and the curing time is 1-1.5 h.
[0013] Preferably, the impregnation pressure of the impregnation treatment is 10-15 MPa, and the impregnation time is 20-30 min; the impregnating agent is a mixture of polyimide fiber and bismaleimide resin in a weight ratio of 2:1.
[0014] Preferably, the mass fraction of the sodium silicate solution is 10-15%; the mass fraction of the sodium lignin sulfonate solution is 8-12%.
[0015] Preferably, the immersion pressure of the immersion treatment is 10-15 MPa, and the immersion time is 20-30 min.
[0016] Preferably, the modification method of the modified nano-silica agent is:
[0017] The nano-silica is first irradiated in a proton irradiation box for 10-15 minutes at an irradiation power of 350W. After the irradiation is completed, 3-5 parts of irradiated nano-silica, 1-3 parts of 5% chitosan solution by mass, 2-5 parts of yttrium oxide, and 1-2 parts of stearic acid are mixed and ball-milled at a ball-milling speed of 1500r / min for 2h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a modified nano-silica agent.
[0018] Preferably, the preparation method of the nano mica agent is:
[0019] S01: heat-treat the nano-mica powder at 150-170°C for 5-10 minutes, then heat it to 275-285°C at a rate of 1-3°C / min, keep it warm for 5 minutes, and finally air-cool it to room temperature;
[0020] S02: Mix the nano-mica powder of S01 with a sufficient amount of sodium citrate solution, and then continue to sinter at 210°C for 5 minutes, and finally air-cool to room temperature.
[0021] Preferably, the mass fraction of the sodium citrate solution is 10-15%.
[0022] The method for preparing a multilayer imide sintered winding round wire for a submersible motor of the present embodiment comprises the following steps:
[0023] The organic silicon resin, m-phenylenediamine, an efficiency regulator, xylene and a nano-mica agent are fully mixed to obtain an insulating modified paint;
[0024] The round wire substrate is treated by impregnation with an insulating modified varnish to form an insulating varnish layer, and then a polyimide film is wound around the insulating varnish layer and sintered to form a polyimide film layer. Finally, an impregnating agent is used for coating and then cured to form a modified layer, thereby obtaining a multi-layer imide sintered winding round wire.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] The sintered winding round wire of the present invention adopts a round wire substrate which is first impregnated with an insulating modified paint, then wound with a polyimide film and sintered to form a polyimide film layer, finally coated with an impregnating agent, and then solidified to form an improved layer. Through multi-layer improvement, the insulation and wear resistance of the product, as well as the acid corrosion resistance stability of the product are optimized; the insulating modified paint adopts an effect-adjusting agent and a nano-mica agent to adjust the effect of each other, and the insulating modified paint product formed by raw materials such as silicone resin and metaphenylenediamine is coordinated to optimize the performance effect of the product. DETAILED DESCRIPTION
[0027] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] The present embodiment is a multi-layer imide sintered winding round wire for a submersible motor, wherein the sintered winding round wire comprises a round wire substrate, the round wire substrate is firstly treated with an insulating modified paint to form an insulating paint layer, and then a polyimide film is wound around the insulating paint layer and sintered to form a polyimide film layer, and finally an impregnating agent is used for coating, and then cured to form a modified layer, so as to obtain a multi-layer imide sintered winding round wire;
[0029] The insulating modified paint comprises the following raw materials in parts by weight:
[0030] 25-30 parts of organic silicon resin, 2-5 parts of meta-phenylenediamine, 5-8 parts of performance regulator, 20-25 parts of xylene, 4-7 parts of nano-mica agent.
[0031] The sintering process temperature of this embodiment is 200-230° C., and the sintering time is 2-5 minutes; the curing temperature is 155-165° C., and the curing time is 1-1.5 hours.
[0032] The impregnation pressure of the impregnation treatment in this embodiment is 10-15 MPa, and the impregnation time is 20-30 min; the impregnation agent is a mixture of polyimide fiber and bismaleimide resin in a weight ratio of 2:1.
[0033] The preparation method of the performance modifier of this embodiment is:
[0034] S1: immersing the glass fiber into a sufficient amount of sodium silicate solution for immersion treatment, and then filtering and drying to obtain an immersed glass fiber agent;
[0035] S2: 2-5 parts of modified nano-silica agent, 3-5 parts of sodium lignin sulfonate solution, 1-3 parts of silane coupling agent KH560 and 4-7 parts of 5% by mass lanthanum nitrate solution are fully mixed to obtain a nano-silica conditioning solution;
[0036] S3: The immersed glass fiber agent and nano-silicon dioxide conditioning solution are mixed in a weight ratio of 5:3 and ball-milled at a ball-milling speed of 1000-1500 r / min for 2 hours. After the ball-milling is completed, the mixture is washed with water and dried to obtain a conditioning agent.
[0037] The mass fraction of the sodium silicate solution in this embodiment is 10-15%; the mass fraction of the sodium lignin sulfonate solution is 8-12%.
[0038] The immersion pressure of the immersion treatment in this embodiment is 10-15 MPa, and the immersion time is 20-30 min.
[0039] The modification method of the modified nano silicon dioxide agent of this embodiment is:
[0040] The nano-silica is first irradiated in a proton irradiation box for 10-15 minutes at an irradiation power of 350W. After the irradiation is completed, 3-5 parts of irradiated nano-silica, 1-3 parts of 5% chitosan solution by mass, 2-5 parts of yttrium oxide, and 1-2 parts of stearic acid are mixed and ball-milled at a ball-milling speed of 1500r / min for 2h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a modified nano-silica agent.
[0041] The preparation method of the nano-mica agent of this embodiment is:
[0042] S01: heat-treat the nano-mica powder at 150-170°C for 5-10 minutes, then heat it to 275-285°C at a rate of 1-3°C / min, keep it warm for 5 minutes, and finally air-cool it to room temperature;
[0043] S02: Mix the nano-mica powder of S01 with a sufficient amount of sodium citrate solution, and then continue to sinter at 210°C for 5 minutes, and finally air-cool to room temperature.
[0044] The mass fraction of the sodium citrate solution of the present embodiment is 10-15%.
[0045] The method for preparing a multilayer imide sintered winding round wire for a submersible motor of the present embodiment comprises the following steps:
[0046] The organic silicon resin, m-phenylenediamine, an efficiency regulator, xylene and a nano-mica agent are fully mixed to obtain an insulating modified paint;
[0047] The round wire substrate is treated by impregnation with an insulating modified varnish to form an insulating varnish layer, and then a polyimide film is wound around the insulating varnish layer and sintered to form a polyimide film layer. Finally, an impregnating agent is used for coating and then cured to form a modified layer, thereby obtaining a multi-layer imide sintered winding round wire. Example 1
[0048] The present embodiment is a multi-layer imide sintered winding round wire for a submersible motor, wherein the sintered winding round wire comprises a round wire substrate, the round wire substrate is firstly treated with an insulating modified paint to form an insulating paint layer, and then a polyimide film is wound around the insulating paint layer and sintered to form a polyimide film layer, and finally an impregnating agent is used for coating, and then cured to form a modified layer, so as to obtain a multi-layer imide sintered winding round wire;
[0049] The insulating modified paint comprises the following raw materials in parts by weight:
[0050] 25 parts of silicone resin, 2 parts of m-phenylenediamine, 5 parts of conditioning agent, 20 parts of xylene, and 4 parts of nano-mica agent.
[0051] The sintering process temperature of this embodiment is 200° C., and the sintering time is 2 minutes; the curing temperature is 155° C., and the curing time is 1 hour.
[0052] The impregnation pressure of the impregnation treatment in this embodiment is 10 MPa, and the impregnation time is 20 min; the impregnation agent is a mixture of polyimide fiber and bismaleimide resin in a weight ratio of 2:1.
[0053] The preparation method of the performance modifier of this embodiment is:
[0054] S1: immersing the glass fiber into a sufficient amount of sodium silicate solution for immersion treatment, and then filtering and drying to obtain an immersed glass fiber agent;
[0055] S2: 2 parts of modified nano-silica agent, 3 parts of sodium lignin sulfonate solution, 1 part of silane coupling agent KH560 and 4 parts of 5% by mass lanthanum nitrate solution are fully mixed to obtain a nano-silica conditioning solution;
[0056] S3: The immersed glass fiber agent and nano-silicon dioxide conditioning liquid are mixed in a weight ratio of 5:3 and ball-milled at a ball-milling speed of 1000 r / min for 2 h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a conditioning agent.
[0057] The mass fraction of the sodium silicate solution in this embodiment is 10%; the mass fraction of the sodium lignin sulfonate solution is 8%.
[0058] The immersion pressure of the immersion treatment in this embodiment is 10 MPa, and the immersion time is 20 minutes.
[0059] The modification method of the modified nano silicon dioxide agent of this embodiment is:
[0060] The nano-silica was first irradiated in a proton irradiation box for 10 minutes at an irradiation power of 350 W. After the irradiation was completed, 3 parts of irradiated nano-silica, 1 part of 5% chitosan solution by mass, 2 parts of yttrium oxide, and 1 part of stearic acid were blended and ball-milled at a ball-milling speed of 1500 r / min for 2 hours. After the ball-milling was completed, the mixture was washed with water and dried to obtain a modified nano-silica agent.
[0061] The preparation method of the nano-mica agent of this embodiment is:
[0062] S01: The nano-mica powder was first heat treated at 150°C for 5 min, then heated to 275°C at a rate of 1°C / min, kept at this temperature for 5 min, and finally air-cooled to room temperature;
[0063] S02: Mix the nano-mica powder of S01 with a sufficient amount of sodium citrate solution, and then continue to sinter at 210°C for 5 minutes, and finally air-cool to room temperature.
[0064] The mass fraction of the sodium citrate solution in this embodiment is 10%.
[0065] The method for preparing a multilayer imide sintered winding round wire for a submersible motor of the present embodiment comprises the following steps:
[0066] The organic silicon resin, m-phenylenediamine, an efficiency regulator, xylene and a nano-mica agent are fully mixed to obtain an insulating modified paint;
[0067] The round wire substrate is treated by impregnation with an insulating modified varnish to form an insulating varnish layer, and then a polyimide film is wound around the insulating varnish layer and sintered to form a polyimide film layer. Finally, an impregnating agent is used for coating and then cured to form a modified layer, thereby obtaining a multi-layer imide sintered winding round wire. Example 2
[0068] The present embodiment is a multi-layer imide sintered winding round wire for a submersible motor, wherein the sintered winding round wire comprises a round wire substrate, the round wire substrate is firstly treated with an insulating modified paint to form an insulating paint layer, and then a polyimide film is wound around the insulating paint layer and sintered to form a polyimide film layer, and finally an impregnating agent is used for coating, and then cured to form a modified layer, so as to obtain a multi-layer imide sintered winding round wire;
[0069] The insulating modified paint comprises the following raw materials in parts by weight:
[0070] 30 parts of organic silicone resin, 5 parts of m-phenylenediamine, 8 parts of performance regulator, 25 parts of xylene, and 7 parts of nano-mica agent.
[0071] The sintering process temperature of this embodiment is 230° C., and the sintering time is 5 minutes; the curing temperature is 165° C., and the curing time is 1.5 hours.
[0072] The impregnation pressure of the impregnation treatment in this embodiment is 15 MPa, and the impregnation time is 30 min; the impregnation agent is a mixture of polyimide fiber and bismaleimide resin in a weight ratio of 2:1.
[0073] The preparation method of the performance modifier of this embodiment is:
[0074] S1: immersing the glass fiber into a sufficient amount of sodium silicate solution for immersion treatment, and then filtering and drying to obtain an immersed glass fiber agent;
[0075] S2: 5 parts of modified nano-silica agent, 5 parts of sodium lignin sulfonate solution, 3 parts of silane coupling agent KH560 and 7 parts of 5% by mass lanthanum nitrate solution are fully mixed to obtain a nano-silica conditioning solution;
[0076] S3: The immersed glass fiber agent and nano-silica conditioning liquid are mixed in a weight ratio of 5:3 and ball-milled at a ball-milling speed of 1500 r / min for 2 h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a conditioning agent.
[0077] The mass fraction of the sodium silicate solution in this embodiment is 15%; the mass fraction of the sodium lignin sulfonate solution is 12%.
[0078] The immersion pressure of the immersion treatment in this embodiment is 15 MPa, and the immersion time is 30 minutes.
[0079] The modification method of the modified nano silicon dioxide agent of this embodiment is:
[0080] The nano-silica was first irradiated in a proton irradiation box for 15 minutes at an irradiation power of 350 W. After the irradiation was completed, 5 parts of irradiated nano-silica, 3 parts of 5% chitosan solution by mass, 5 parts of yttrium oxide, and 2 parts of stearic acid were blended and ball-milled at a ball-milling speed of 1500 r / min for 2 hours. After the ball-milling was completed, the mixture was washed with water and dried to obtain a modified nano-silica agent.
[0081] The preparation method of the nano-mica agent of this embodiment is:
[0082] S01: The nano-mica powder was first heat treated at 170°C for 10 min, then heated to 285°C at a rate of 3°C / min, kept at this temperature for 5 min, and finally air-cooled to room temperature;
[0083] S02: Mix the nano-mica powder of S01 with a sufficient amount of sodium citrate solution, and then continue to sinter at 210°C for 5 minutes, and finally air-cool to room temperature.
[0084] The mass fraction of the sodium citrate solution in this embodiment is 15%.
[0085] The method for preparing a multilayer imide sintered winding round wire for a submersible motor of the present embodiment comprises the following steps:
[0086] The organic silicon resin, m-phenylenediamine, an efficiency regulator, xylene and a nano-mica agent are fully mixed to obtain an insulating modified paint;
[0087] The round wire substrate is treated by impregnation with an insulating modified varnish to form an insulating varnish layer, and then a polyimide film is wound around the insulating varnish layer and sintered to form a polyimide film layer. Finally, an impregnating agent is used for coating and then cured to form a modified layer, thereby obtaining a multi-layer imide sintered winding round wire. Example 3
[0088] The present embodiment is a multi-layer imide sintered winding round wire for a submersible motor, wherein the sintered winding round wire comprises a round wire substrate, the round wire substrate is firstly treated with an insulating modified paint to form an insulating paint layer, and then a polyimide film is wound around the insulating paint layer and sintered to form a polyimide film layer, and finally an impregnating agent is used for coating, and then cured to form a modified layer, so as to obtain a multi-layer imide sintered winding round wire;
[0089] The insulating modified paint comprises the following raw materials in parts by weight:
[0090] 27.5 parts of organic silicon resin, 3.5 parts of m-phenylenediamine, 6.5 parts of performance regulator, 22.5 parts of xylene, and 5.5 parts of nano-mica agent.
[0091] The sintering process temperature of this embodiment is 215° C., and the sintering time is 3.5 minutes; the curing temperature is 160° C., and the curing time is 1.2 hours.
[0092] The impregnation pressure of the impregnation treatment in this embodiment is 12 MPa, and the impregnation time is 25 min; the impregnation agent is a mixture of polyimide fiber and bismaleimide resin in a weight ratio of 2:1.
[0093] The preparation method of the performance modifier of this embodiment is:
[0094] S1: immersing the glass fiber into a sufficient amount of sodium silicate solution for immersion treatment, and then filtering and drying to obtain an immersed glass fiber agent;
[0095] S2: 3.5 parts of modified nano-silica agent, 4 parts of sodium lignin sulfonate solution, 2 parts of silane coupling agent KH560 and 5.5 parts of 5% by mass lanthanum nitrate solution are fully mixed to obtain a nano-silica conditioning solution;
[0096] S3: The immersed glass fiber agent and nano-silicon dioxide conditioning solution are mixed in a weight ratio of 5:3 and ball-milled at a ball-milling speed of 1250 r / min for 2 h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a conditioning agent.
[0097] The mass fraction of the sodium silicate solution in this embodiment is 12.5%; the mass fraction of the sodium lignin sulfonate solution is 10%.
[0098] The immersion pressure of the immersion treatment in this embodiment is 12.5 MPa, and the immersion time is 25 minutes.
[0099] The modification method of the modified nano silicon dioxide agent of this embodiment is:
[0100] The nano-silica was first irradiated in a proton irradiation box for 12.5 minutes at an irradiation power of 350 W. After the irradiation was completed, 4 parts of irradiated nano-silica, 2 parts of 5% chitosan solution by mass, 3.5 parts of yttrium oxide, and 1.5 parts of stearic acid were blended and ball-milled at a ball-milling speed of 1500 r / min for 2 hours. After the ball-milling was completed, the mixture was washed with water and dried to obtain a modified nano-silica agent.
[0101] The preparation method of the nano-mica agent of this embodiment is:
[0102] S01: The nano-mica powder was first heat treated at 160°C for 7.5 min, then heated to 280°C at a rate of 2°C / min, kept at this temperature for 5 min, and finally air-cooled to room temperature;
[0103] S02: Mix the nano-mica powder of S01 with a sufficient amount of sodium citrate solution, and then continue to sinter at 210°C for 5 minutes, and finally air-cool to room temperature.
[0104] The mass fraction of the sodium citrate solution in this embodiment is 12.5%.
[0105] The method for preparing a multilayer imide sintered winding round wire for a submersible motor of the present embodiment comprises the following steps:
[0106] The organic silicon resin, m-phenylenediamine, an efficiency regulator, xylene and a nano-mica agent are fully mixed to obtain an insulating modified paint;
[0107] The round wire substrate is treated by impregnation with an insulating modified varnish to form an insulating varnish layer, and then a polyimide film is wound around the insulating varnish layer and sintered to form a polyimide film layer. Finally, an impregnating agent is used for coating and then cured to form a modified layer, thereby obtaining a multi-layer imide sintered winding round wire.
[0108] Comparative Example 1
[0109] The difference from Example 3 is that no conditioning agent is added to the insulation modified paint.
[0110] Comparative Example 2
[0111] The difference from Example 3 is that the nano-silicon dioxide conditioning liquid is not used in the preparation of the conditioning agent.
[0112] Comparative Example 3
[0113] The difference from Example 3 is that no modified nano-silica agent is added to the nano-silica conditioning solution.
[0114] Comparative Example 4
[0115] The difference from Example 3 is that the modified nano-silica agent is replaced by nano-silica.
[0116] Comparative Example 5
[0117] The difference from Example 3 is that no nano mica agent is added.
[0118] The products of Examples 1-3 and Comparative Examples 1-5 of the present invention were subjected to performance tests, and the products were placed in a 2% hydrochloric acid acid corrosion condition for 12 hours to test the acid corrosion resistance stability of the products;
[0119]
[0120] It can be seen from Examples 1-3 and Comparative Examples 1-5 that the products of Examples 1-3 of the present invention have excellent insulation and wear resistance, and the performance of the two is improved in a coordinated manner, and the acid corrosion resistance stability of the products is remarkable; no performance-adjusting agent and no nano-mica agent are added to the insulation modified paint, and the performance of the products has a significant trend of deterioration. At the same time, the performance-adjusting agent is not treated with nano-silicon dioxide regulating liquid in the preparation of the performance-adjusting agent, and the modified nano-silicon dioxide agent is not added to the nano-silicon dioxide regulating liquid. The modified nano-silicon dioxide agent is replaced by nano-silicon dioxide, and the performance of the products has a trend of deterioration. Only when the performance-adjusting agent obtained by the method of the present invention is combined with the nano-mica agent, the performance effect of the product is the most significant, and the replacement by other methods is not as significant as the effect of the present invention.
[0121] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0122] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A multilayer imide sintered winding round wire for a submersible motor, the sintered winding round wire comprising a round wire matrix, It is characterized in that The round wire substrate is firstly treated with an insulating modified paint to form an insulating paint layer, and then a polyimide film is wound around the insulating paint layer and sintered to form a polyimide film layer, and finally an impregnating agent is used for coating, and then cured to form a modified layer, so as to obtain a multi-layer imide sintered winding round wire; The insulating modified paint comprises the following raw materials in parts by weight: 25-30 parts of organic silicon resin, 2-5 parts of m-phenylenediamine, 5-8 parts of conditioning agent, 20-25 parts of xylene, 4-7 parts of nano-mica agent; The impregnation pressure of the impregnation treatment is 10-15MPa, and the impregnation time is 20-30min; the impregnation agent is a mixture of polyimide fiber and bismaleimide resin in a weight ratio of 2:1; the preparation method of the performance modifier is: S1: immersing the glass fiber into a sufficient amount of sodium silicate solution for immersion treatment, and then filtering and drying to obtain an immersed glass fiber agent; S2: 2-5 parts of modified nano-silica agent, 3-5 parts of sodium lignin sulfonate solution, 1-3 parts of silane coupling agent KH560 and 4-7 parts of 5% by mass lanthanum nitrate solution are fully mixed to obtain a nano-silica conditioning solution; S3: The immersed glass fiber agent and nano-silicon dioxide conditioning solution are mixed and ball-milled in a weight ratio of 5:3, with a ball-milling speed of 1000-1500 r / min for 2 h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a conditioning agent; The modification method of the modified nano silicon dioxide agent is: The nano-silicon dioxide is first irradiated in a proton irradiation box for 10-15 minutes, the irradiation power is 350W, and after the irradiation is completed, 3-5 parts of the irradiated nano-silicon dioxide, 1-3 parts of a chitosan solution with a mass fraction of 5%, 2-5 parts of yttrium oxide, and 1-2 parts of stearic acid are mixed and ball-milled at a ball-milling speed of 1500r / min for 2h. After the ball-milling is completed, the modified nano-silicon dioxide agent is washed with water and dried to obtain the modified nano-mica agent; the preparation method of the nano-mica agent is as follows: S01: heat-treat the nano-mica powder at 150-170°C for 5-10 minutes, then heat it to 275-285°C at a rate of 1-3°C / min, keep it warm for 5 minutes, and finally air-cool it to room temperature; S02: Mix the nano-mica powder of S01 with a sufficient amount of sodium citrate solution, and then continue to sinter at 210°C for 5 minutes, and finally air-cool to room temperature.
2. A multilayer imide sintered winding round wire for a submersible motor according to claim 1, It is characterized in that The sintering temperature is 200-230° C., and the sintering time is 2-5 minutes; the curing temperature is 155-165° C., and the curing time is 1-1.5 hours.
3. The multilayer imide sintered winding round wire for a submersible motor according to claim 1, It is characterized in that The mass fraction of the sodium silicate solution is 10-15%; the mass fraction of the sodium lignin sulfonate solution is 8-12%.
4. The multilayer imide sintered winding round wire for a submersible motor according to claim 1, It is characterized in that The immersion pressure of the immersion treatment is 10-15 MPa, and the immersion time is 20-30 min.
5. The multilayer imide sintered winding round wire for a submersible motor according to claim 1, It is characterized in that The mass fraction of the sodium citrate solution is 10-15%.
6. A method for preparing a multilayer imide sintered winding round wire for a submersible motor as claimed in any one of claims 1 to 5, It is characterized in that The following steps are involved: The organic silicon resin, m-phenylenediamine, an efficiency regulator, xylene and a nano-mica agent are fully mixed to obtain an insulating modified paint; The round wire substrate is treated by impregnation with an insulating modified varnish to form an insulating varnish layer, and then a polyimide film is wound around the insulating varnish layer and sintered to form a polyimide film layer. Finally, an impregnating agent is used for coating and then cured to form a modified layer, thereby obtaining a multi-layer imide sintered winding round wire.