A high short-circuit current back contact battery and preparation method thereof and photovoltaic module

By setting the phosphorus-doped hydrogen-doped region and anti-reverse layer on the front of the silicon wafer of the back contact battery, combined with the conductive film layer structure, the short circuit caused by the N-type polycrystalline silicon layer/N-type amorphous silicon layer in the prior art is solved. The problems of low current and open circuit voltage drop have achieved the consideration of high short circuit current and high open circuit voltage.

CN118507546BActive Publication Date: 2024-11-08GOLD STONE (FUJIAN) ENERGY CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410955587.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-08
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

The existing back contact heterojunction solar cells have severe parasitic absorption losses of the N-type polysilicon layer/N-type amorphous silicon layer, resulting in low short-circuit current. At the same time, canceling these layers will lead to a decrease in the open circuit voltage.

Method used

By setting the phosphorus-doped hydrogen doped region on the oxide layer on the front of the silicon wafer, the field passivation effect is provided, and the N-type polysilicon layer/N-type amorphous silicon layer is eliminated, and the phosphorus-doped hydrogen doped region with specific thickness and doping concentration is adopted. , combined with the anti-reverse layer and conductive film layer structure, the passivation level is improved to increase the open circuit voltage and short circuit current.

Benefits of technology

It realizes the reduction of optical loss while maintaining a high open circuit voltage, and improves the short circuit current of the back contact battery, solving the problems of low short circuit current and open circuit voltage drop.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118507546B_ABST
    Figure CN118507546B_ABST
Patent Text Reader

Abstract

The invention discloses a back-contact cell with high short-circuit current, a preparation method thereof and a photovoltaic module, and relates to the technical field of back-contact cells. The back-contact cell with high short-circuit current comprises a silicon wafer, an oxide layer and an anti-reflection layer arranged in sequence on the front side of the silicon wafer, a phosphorus-doped and hydrogen-doped region is arranged on one side of the oxide layer close to the anti-reflection layer, wherein the depth of the phosphorus-doped and hydrogen-doped region is 1.6nm-3nm, and the phosphorus doping concentration is 1e18cm ‑3 ‑5e18cm ‑3 , the hydrogen content is 5e18cm ‑3 ‑8e18cm ‑3 The high short-circuit current back-contact cell provided by the present invention can provide a field passivation effect, passivate surface defects, and improve the passivation level, so that the back-contact cell maintains a higher open-circuit voltage, and eliminates the N-type polysilicon layer / N-type amorphous silicon layer, which can reduce optical losses to a minimum, so that the back-contact cell has a higher short-circuit current.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of back contact batteries, and in particular relates to a back contact battery with high short-circuit current, a preparation method thereof, and a photovoltaic module. Background Art

[0002] Existing back-contact heterojunction solar cells usually use a tunneling oxide layer plus an N-type polysilicon layer structure (or an intrinsic amorphous silicon layer plus an N-type amorphous silicon layer structure) on the front side. Since the parasitic absorption loss of the N-type polysilicon layer / N-type amorphous silicon layer is serious, the short-circuit current of the entire back-contact battery is relatively low. Since the N-type polysilicon layer / N-type amorphous silicon layer mainly provides a field passivation effect, if the N-type polysilicon layer / N-type amorphous silicon layer is eliminated, the open-circuit voltage will be significantly reduced.

[0003] It should be noted that this part of the present invention only provides background technology related to the present invention and does not necessarily constitute prior art or known technology. Summary of the invention

[0004] The purpose of the present invention is to overcome the defects of the prior art that the back-contact battery has serious parasitic absorption loss on the front side and low short-circuit current, and to provide a back-contact battery with high short-circuit current and a preparation method and a photovoltaic module thereof. The back-contact battery provides a field passivation effect through the phosphorus-doped and hydrogen-doped regions on the oxide layer, effectively passivates surface defects, improves the passivation level, and allows the back-contact battery to maintain a higher open-circuit voltage. The N-type polysilicon layer / N-type amorphous silicon layer is eliminated, which can reduce optical losses to a minimum, so that the back-contact battery has a higher short-circuit current.

[0005] In order to achieve the above-mentioned object, in the first aspect, the present invention provides a back contact battery with high short-circuit current, comprising a silicon wafer, and an oxide layer and an anti-reflection layer sequentially arranged on the front side of the silicon wafer, wherein a phosphorus-doped and hydrogen-doped region is arranged on the side of the oxide layer close to the anti-reflection layer, wherein the depth of the phosphorus-doped and hydrogen-doped region is 1.6nm-3nm, and the phosphorus doping concentration is 1e18cm -3 -5e18cm -3 , the hydrogen content is 5e18cm -3 -8e18cm -3 .

[0006] Preferably, the thickness of the oxide layer is 4 nm-6 nm; and / or the thickness of the anti-reflection layer is 80 nm-110 nm.

[0007] Preferably, the anti-reflection layer is selected from at least one of silicon nitride, silicon oxynitride and silicon oxide; and / or the refractive index of the anti-reflection layer is 2.2-2.5.

[0008] Preferably, the high short-circuit current back-contact battery also includes a first semiconductor layer and a second semiconductor layer simultaneously arranged on the back side of the silicon wafer, the first semiconductor layer is provided with a first opening area, a portion of the second semiconductor layer covers the side of the first semiconductor layer away from the silicon wafer, and the other portion extends into the first opening area and covers the silicon wafer.

[0009] Preferably, the back-contact battery with high short-circuit current also includes a conductive film layer, which is arranged on the side of the first semiconductor layer and the second semiconductor layer away from the silicon wafer, and the second semiconductor layer is provided with a second opening area, and the second opening areas are alternately and spaced apart from the first opening areas, a part of the conductive film layer extends into the first opening area and covers the second semiconductor layer, and another part extends into the second opening area and covers the first semiconductor layer, and an isolation groove is provided between two adjacent parts of the conductive film layer.

[0010] Preferably, the high short-circuit current back-contact battery further comprises a first electrode and a second electrode, wherein the first electrode is arranged on the portion of the conductive film layer extending into the first opening region, and the second electrode is arranged on the portion of the conductive film layer extending into the second opening region.

[0011] Preferably, the first semiconductor layer includes a tunneling silicon oxide layer and a first doping layer, the first doping layer is arranged on a side of the tunneling silicon oxide layer away from the silicon wafer, the thickness of the tunneling silicon oxide layer is 1nm-2nm, the thickness of the first doping layer is 150nm-300nm, and the phosphorus doping concentration in the first doping layer is 1e20cm -3 -5e20cm -3 , the carbon doping concentration in the first doping layer is 1e19cm -3 -8e19cm -3 .

[0012] Preferably, the second semiconductor layer includes an intrinsic amorphous silicon layer and a second doped layer, the second doped layer is arranged on a side of the intrinsic amorphous silicon layer away from the silicon wafer, the thickness of the intrinsic amorphous silicon layer is 5nm-15nm, the thickness of the second doped layer is 10nm-35nm, and the boron doping concentration in the second doped layer is 1e19cm -3 -4e20cm -3 .

[0013] In a second aspect, the present invention provides a method for preparing a back contact battery, which is used to prepare the above-mentioned back contact battery with high short-circuit current. The method for preparing the back contact battery with high short-circuit current comprises the following steps:

[0014] S1. Polishing and cleaning the back side of the silicon wafer;

[0015] S2. sequentially forming a first semiconductor layer and a mask layer on the back side of the silicon wafer;

[0016] S3. annealing the first semiconductor layer;

[0017] S4. Etching an opening on the first semiconductor layer and the mask layer to form a first opening region;

[0018] S5. The first semiconductor layer and the mask layer remaining in the first opening region are removed by texturing and cleaning, and a velvet surface is formed on the front side of the silicon wafer and in the first opening region; thereafter, the mask layer outside the first opening region is removed by cleaning;

[0019] S6. forming an oxide layer and an anti-reflection layer on the front side of the silicon wafer in sequence; wherein, firstly, introducing nitrous oxide and performing oxidation under the condition of turning on the glow to form an oxide layer; then introducing a mixed gas of 2% phosphine and 98% hydrogen, and performing phosphorus-doped and hydrogen-doped treatment on the oxide layer under the condition of turning on the glow to form a phosphorus-doped and hydrogen-doped region on the oxide layer; then introducing silane and ammonia, and forming an anti-reflection layer under the condition of turning on the glow;

[0020] S7. Form a second semiconductor layer on the back side of the silicon wafer, so that a portion of the second semiconductor layer covers the side of the first semiconductor layer away from the silicon wafer, and another portion of the second semiconductor layer extends into the first opening area and covers the silicon wafer.

[0021] Preferably, in S6, the reaction conditions for forming the oxide layer are: reaction temperature of 400°C-450°C, nitrous oxide flow rate of 5000sccm-8000sccm, reaction pressure of 1000mtorr-3000mtorr, reaction time of 240s-360s, and reaction power of 4kW-6kW;

[0022] and / or, the reaction conditions for forming the phosphorus-doped and hydrogen-doped regions are: reaction temperature of 400° C.-450° C., phosphine flow rate of 300 sccm-500 sccm, reaction pressure of 100 mtorr-300 mtorr, reaction time of 120 s-240 s, and reaction power of 1.5 kW-3 kW;

[0023] And / or, the reaction conditions for forming the anti-reflection layer are: reaction temperature of 400°C-450°C, silane flow rate of 1200sccm-1600sccm, ammonia flow rate of 5000sccm-8000sccm, reaction pressure of 500mtorr-3000mtorr, reaction time of 700s-1000s, and reaction power of 4kW-6kW.

[0024] Preferably, after S7, the method for preparing a back contact battery with a high short-circuit current further comprises:

[0025] S8. Etching openings on the second semiconductor layer to form second opening regions alternately arranged with the first opening regions and spaced apart, followed by cleaning;

[0026] S9. forming a conductive film layer on the back side of the silicon wafer;

[0027] S10. An isolation groove is formed on the conductive film layer so that a portion of the conductive film layer separated from each other extends into the first opening region and covers the second semiconductor layer, and another portion extends into the second opening region and covers the first semiconductor layer;

[0028] S11. Form a first electrode on the portion of the conductive film layer extending into the first opening region, and form a second electrode on the portion of the conductive film layer extending into the second opening region.

[0029] In a third aspect, the present invention provides a photovoltaic module, which includes the above-mentioned high short-circuit current back contact cell.

[0030] Beneficial effects:

[0031] It has been found through research that when the N-type polysilicon layer / N-type amorphous silicon layer is used on the front of the back contact cell, the parasitic absorption loss is serious, which makes the short-circuit current of the back contact cell low. If the N-type polysilicon layer / N-type amorphous silicon layer is directly eliminated, the field passivation effect will be lost, resulting in a significant reduction in the open circuit voltage of the back contact cell. It is well known that the front of the back contact cell does not require electron transmission, and only needs to ensure a high level of passivation and low optical loss. Based on this, further research was conducted to propose the present invention.

[0032] The present invention adopts the above-mentioned technical scheme, especially by arranging a phosphorus-doped and hydrogen-doped region with a specific thickness, a specific phosphorus-doped concentration, and a specific hydrogen-doped concentration on the side of the oxide layer close to the anti-reflection layer, so as to provide a field passivation effect through the phosphorus-doped oxide layer, and at the same time passivate surface defects through the hydrogen-doped oxide layer, thereby further improving the passivation level, so that the back contact battery maintains a relatively high open circuit voltage, wherein the depth of the phosphorus-doped and hydrogen-doped region is appropriate, so as to obtain better field passivation and interface passivation, which is beneficial to improving the open circuit voltage of the battery; and the N-type polysilicon layer / N-type amorphous silicon layer is eliminated, so as to reduce the optical loss to a minimum, so that the back contact battery has a relatively high short circuit current.

[0033] In the preparation method of the present invention, firstly, laughing gas is introduced and oxidized under the condition of turning on the glow to form an oxide layer; then, a mixed gas of 2% phosphine and 98% hydrogen is introduced, and phosphorus-doped and hydrogen-doped treatment is performed on the oxide layer under the condition of turning on the glow to form a phosphorus-doped and hydrogen-doped region on the oxide layer; then, silane and ammonia are introduced, and an anti-reflection layer is formed under the condition of turning on the glow; the phosphorus-doped and hydrogen-doped region is formed on the side of the oxide layer close to the anti-reflection layer, thereby greatly improving the preparation efficiency. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0035] Figure 1 This is a schematic diagram of the structure of a silicon wafer after double-sided polishing and cleaning according to an embodiment of the present invention;

[0036] Figure 2 This is a schematic diagram of the structure of forming a first semiconductor layer and a mask layer on the back side of a silicon wafer according to an embodiment of the present invention;

[0037] Figure 3 This is a schematic diagram of the structure after oxidation annealing in an embodiment of the present invention;

[0038] Figure 4 This is a schematic diagram of the structure of forming a combined anti-reflection layer on the front side of a silicon wafer according to an embodiment of the present invention;

[0039] Figure 5 It is a structural schematic diagram of forming a second semiconductor layer and a second opening area on the back side of a silicon wafer according to an embodiment of the present invention;

[0040] Figure 6 This is a schematic diagram of the structure of depositing a conductive film layer on the back side of a silicon wafer according to an embodiment of the present invention;

[0041] Figure 7 It is a schematic diagram of the structure of forming a metal electrode on the back side of a silicon wafer according to an embodiment of the present invention.

[0042] Description of Reference Numerals

[0043] 1-silicon wafer; 2-tunneling oxide layer; 3-first doping layer; 4-mask layer; 5-oxide layer; 6-phosphorus-doped and hydrogen-doped regions; 7-anti-reflection layer; 8-intrinsic amorphous silicon layer; 9-second doping layer; 10-conductive film layer. DETAILED DESCRIPTION

[0044] In the present invention, unless otherwise specified, directional words such as "upper, lower, left, right" are generally understood in conjunction with the directions shown in the drawings and actual applications.

[0045] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.

[0046] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0047] The endpoints and any values ​​of the ranges disclosed herein are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Among them, the terms "optional" and "optional" all mean that they may be included or not included (or may be present or not).

[0048] In the first aspect, the present invention provides a back-contact cell with high short-circuit current, which provides a field passivation effect through the phosphorus-doped and hydrogen-doped regions on the oxide layer, effectively passivates surface defects, improves the passivation level, and enables the back-contact cell to maintain a relatively high open-circuit voltage. In addition, the N-type polysilicon layer / N-type amorphous silicon layer is eliminated, which can reduce optical losses to a minimum, thereby enabling the back-contact cell to have a relatively high short-circuit current.

[0049] The back contact cell with high short-circuit current includes a silicon wafer and an oxide layer and an anti-reflection layer arranged on the front side of the silicon wafer in sequence. A phosphorus-doped and hydrogen-doped region is arranged on the side of the oxide layer close to the anti-reflection layer. The depth of the phosphorus-doped and hydrogen-doped region is 1.6nm-3nm. A reasonable depth of the phosphorus-doped and hydrogen-doped region can obtain better field passivation and interface passivation, which is conducive to improving the open circuit voltage; the phosphorus doping concentration is 1e18cm -3 -5e18cm -3 , a reasonable phosphorus doping concentration can obtain a better field passivation effect, which is beneficial to improve the open circuit voltage; the hydrogen atomic content is 5e18cm -3 -8e18cm -3 , reasonable hydrogen atom content can achieve better interface passivation, which is beneficial to improving the open circuit voltage.

[0050] In the present invention, the phosphorus-doped and hydrogen-doped region on the oxide layer is obtained after the oxide layer is treated with phosphorus-doped and hydrogen-doped. The depth direction of the phosphorus-doped and hydrogen-doped region is the thickness direction of the oxide layer. The shape and size of the phosphorus-doped and hydrogen-doped region are the same as the shape and size of the oxide layer, that is, the part of the oxide layer that is treated with phosphorus-doped and hydrogen-doped is the phosphorus-doped and hydrogen-doped region, and the part that is not treated with phosphorus-doped and hydrogen-doped is a conventional oxide layer.

[0051] Preferably, the thickness of the oxide layer is 4nm-6nm. A reasonable thickness of the oxide layer can ensure the stable formation of the phosphorus-doped and hydrogen-doped regions, which is beneficial to improving the passivation effect through the phosphorus-doped and hydrogen-doped regions, so that the back contact battery maintains a higher open circuit voltage.

[0052] Preferably, the thickness of the anti-reflection layer is 80 nm-110 nm. A reasonable thickness of the anti-reflection layer can reduce the reflection of light to the maximum extent, which is beneficial to improving the short-circuit current.

[0053] Preferably, the anti-reflection layer is selected from at least one of silicon nitride, silicon oxynitride and silicon oxide.

[0054] Preferably, the refractive index of the anti-reflection layer is 2.2-2.5. A reasonable refractive index of the anti-reflection layer can maximize the absorption of light and help increase the short-circuit current.

[0055] In some preferred embodiments of the present invention, the back-contact battery with high short-circuit current further comprises a first semiconductor layer and a second semiconductor layer disposed simultaneously on the back side of the silicon wafer. The first semiconductor layer is provided with a first opening region, a portion of the second semiconductor layer covers a side of the first semiconductor layer away from the silicon wafer, and another portion of the second semiconductor layer extends into the first opening region and covers the silicon wafer.

[0056] Specifically, there are multiple first opening areas, and the multiple first opening areas are arranged at intervals to divide the first semiconductor layer into multiple sections. A portion of the second semiconductor layer covers the side of the first semiconductor layer away from the silicon wafer, and another portion extends into the first opening area and covers the silicon wafer exposed due to the opening of the first opening area.

[0057] Preferably, the first semiconductor layer includes a tunneling silicon oxide layer and a first doping layer, and the first doping layer is arranged on the side of the tunneling silicon oxide layer away from the silicon wafer. The first doping layer is an N-type doped polysilicon layer, the thickness of the tunneling silicon oxide layer is 1nm-2nm, the thickness of the first doping layer is 150nm-300nm, and the phosphorus doping concentration in the first doping layer is 1e20cm -3 -5e20cm -3 The reasonable phosphorus doping concentration in the first doping layer can provide a good field passivation effect, which is beneficial to improve the open circuit voltage. The carbon doping concentration in the first doping layer is 1e19cm -3 -8e19cm -3 ,A reasonable carbon doping concentration in the first doping layer can reduce the sacrificial absorption of the back polycrystalline and increase the corrosion resistance, which is beneficial to improving the short-circuit current and fill factor.

[0058] Preferably, the second semiconductor layer includes an intrinsic amorphous silicon layer and a second doped layer, and the second doped layer is arranged on a side of the intrinsic amorphous silicon layer away from the silicon wafer. The second doped layer is a P-type doped amorphous or microcrystalline silicon layer, the thickness of the intrinsic amorphous silicon layer is 5nm-15nm, the thickness of the second doped layer is 10nm-35nm, and the boron doping concentration in the second doped layer is 1e19cm -3 -4e20cm -3 , a reasonable boron doping concentration in the second doping layer can provide a better field passivation effect, which is beneficial to improving the open circuit voltage.

[0059] In some preferred embodiments of the present invention, the back contact battery with high short-circuit current further comprises a conductive film layer, which is arranged on the side of the first semiconductor layer and the second semiconductor layer away from the silicon wafer. The second semiconductor layer is provided with a second opening area, which is alternately and spaced apart from the first opening area, a part of the conductive film layer extends into the first opening area and covers the second semiconductor layer, and another part extends into the second opening area and covers the first semiconductor layer, and an isolation groove is provided between two adjacent parts of the conductive film layer, and the isolation groove is used to achieve the insulation function between the two adjacent parts of the conductive film layer.

[0060] Specifically, there are a plurality of second opening areas, and the plurality of second opening areas are arranged at intervals to divide the second semiconductor layer into a plurality of sections. The plurality of first opening areas and the plurality of second opening areas are arranged alternately in sequence, a portion of the conductive film layer extends into the first opening area and covers the second semiconductor layer located in the first opening area, and another portion extends into the second opening area and covers the first semiconductor layer exposed due to the opening of the second opening area. Accordingly, there are a plurality of isolation grooves, and each isolation groove is located between a first opening area and a second opening area adjacent thereto.

[0061] The widths of the first opening area, the second opening area and the isolation groove can be determined according to the range of the prior art and actual needs. For example, the width S102 of the first opening area can be 0.3mm-0.6mm, the width S101 of the second opening area can be 0.1mm-0.3mm, and the width of the isolation groove can be 30μm-200μm.

[0062] In some preferred embodiments of the present invention, the back contact battery with high short-circuit current further comprises a first electrode and a second electrode, wherein the first electrode is arranged on a portion of the conductive film layer extending into the first opening area, and is connected to the second semiconductor layer through the conductive film layer; the second electrode is arranged on a portion of the conductive film layer extending into the second opening area, and is connected to the first semiconductor layer through the conductive film layer.

[0063] The thickness and type of the conductive film layer can refer to the range of the prior art. For example, the thickness of the conductive film layer is 40nm-80nm, and the material of the conductive film layer can be an indium oxide film doped with tin oxide, titanium oxide, zinc oxide or gallium oxide, or a zinc oxide film doped with aluminum oxide, gallium oxide or boron oxide.

[0064] In a second aspect, the present invention provides a method for preparing a back contact battery, which is used to prepare the above-mentioned back contact battery with high short-circuit current. The method for preparing the back contact battery with high short-circuit current comprises the following steps:

[0065] S1. Polishing and cleaning the back side of the silicon wafer;

[0066] S2. sequentially forming a first semiconductor layer and a mask layer on the back side of the silicon wafer;

[0067] S3. annealing the first semiconductor layer;

[0068] S4. Etching an opening on the first semiconductor layer and the mask layer to form a first opening region;

[0069] S5. The first semiconductor layer and the mask layer remaining in the first opening region are removed by texturing and cleaning, and a velvet surface is formed on the front side of the silicon wafer and in the first opening region; thereafter, the mask layer outside the first opening region is removed by cleaning;

[0070] S6. forming an oxide layer and an anti-reflection layer on the front side of the silicon wafer in sequence; wherein, firstly, introducing nitrous oxide and performing oxidation under the condition of turning on the glow to form an oxide layer; then introducing a mixed gas of 2% phosphine and 98% hydrogen, and performing phosphorus-doped and hydrogen-doped treatment on the oxide layer under the condition of turning on the glow to form a phosphorus-doped and hydrogen-doped region on the oxide layer; then introducing silane and ammonia, and forming an anti-reflection layer under the condition of turning on the glow;

[0071] S7. Form a second semiconductor layer on the back side of the silicon wafer, so that a portion of the second semiconductor layer covers the side of the first semiconductor layer away from the silicon wafer, and another portion of the second semiconductor layer extends into the first opening area and covers the silicon wafer.

[0072] It should be noted that, in S1, the silicon wafer is preferably an N-type single crystal silicon wafer, and the silicon wafer can be a Czochralski single crystal silicon wafer or a cast single crystal silicon wafer.

[0073] In S2, the formation of the first semiconductor layer and the mask layer can refer to the method of the prior art, for example, it can be formed by tubular PECVD, LPCVD or PVD in-situ doping deposition annealing, preferably using tubular PECVD in-situ doping. Specifically, in the first stage, laughing gas is introduced, and a tunneling oxide layer is formed by chemical reaction under the condition of turning on the glow. The reaction conditions of the first stage are: reaction temperature of 400℃-450℃, reaction pressure of 100mtorr-2000mtorr, and reaction time of 10s-60s; in the second stage, silane, phosphine and hydrogen are introduced, and a carbon-doped first doping layer is formed by chemical reaction under the condition of turning on the glow. The reaction conditions of the second stage are: reaction temperature of 400℃-450℃, reaction time of 500s-1500s, and reaction pressure of 100mtorr-2000mtorr.

[0074] The type and thickness of the mask layer can refer to the prior art, for example, the type can be at least one of silicon nitride, silicon oxide, silicon oxynitride or nitrogen-containing polysilicon, preferably silicon nitride. The thickness of the mask layer can be 50nm-200nm.

[0075] In S3, nitrogen is introduced to anneal the first semiconductor layer. The annealing conditions are: annealing pressure of 100 mbar-500 mbar, annealing temperature of 850° C.-950° C., nitrogen flow rate of 3000 sccm-10000 sccm, and annealing time of 10 min-60 min.

[0076] In S4, laser or mask etching is used to etch an opening on the first semiconductor layer and the mask layer on the back of the silicon wafer to form a first opening area, and the mask layer, the first doping layer and the tunneling oxide layer in the first opening area are etched away. Laser etching is preferred, and the laser used for etching is an ultraviolet laser or a green laser, and the pulse width is less than 100ns.

[0077] In S5, the mask layer, the first doping layer and the tunneling oxide layer remaining in the first opening area are removed by texturing and cleaning, and a texture surface is formed on the front side of the silicon wafer and in the first opening area. Thereafter, the mask layer outside the first opening area on the back side of the silicon wafer is removed by hydrofluoric acid cleaning.

[0078] In S6, in the first stage, nitrous oxide is introduced, and oxidation is carried out under the condition of turning on the glow to form an oxide layer. The reaction conditions of the first stage are: reaction temperature of 400°C-450°C, nitrous oxide flow rate of 5000sccm-8000sccm, reaction pressure of 1000mtorr-3000mtorr, reaction time of 240s-360s, and reaction power of 4kW-6kW; in the second stage, a mixed gas of 2% phosphine and 98% hydrogen is introduced, and the oxide layer is doped with phosphorus and hydrogen under the condition of turning on the glow to form a phosphorus-doped and hydrogen-doped region on the oxide layer. The reaction conditions of the second stage are: reaction temperature of 400°C-450°C, phosphine flow rate of 5000sccm-8000sccm, reaction pressure of 1000mtorr-3000mtorr, reaction time of 240s-360s, and reaction power of 4kW-6kW. The flow rate is 300sccm-500sccm, the reaction pressure is 100mtorr-300mtorr, the reaction time is 120s-240s, and the reaction power is 1.5kW-3kW; in the third stage, silane and ammonia are introduced, and an anti-reflection layer is formed under the condition of turning on the glow. The reaction conditions of the third stage are: reaction temperature is 400℃-450℃, silane flow rate is 1200sccm-1600sccm, ammonia flow rate is 5000sccm-8000sccm, reaction pressure is 500mtorr-3000mtorr, reaction time is 700s-1000s, and reaction power is 4kW-6kW.

[0079] In S7, a second semiconductor layer is deposited on the back side of the silicon wafer by plasma enhanced chemical vapor deposition (PECVD) technology.

[0080] Preferably, after S7, the method for preparing a back contact battery with a high short-circuit current further comprises:

[0081] S8. Etching openings on the second semiconductor layer to form second opening regions alternately arranged with the first opening regions and spaced apart, followed by cleaning;

[0082] S9. forming a conductive film layer on the back side of the silicon wafer;

[0083] S10. An isolation groove is formed on the conductive film layer so that a portion of the conductive film layer separated from each other extends into the first opening region and covers the second semiconductor layer, and another portion extends into the second opening region and covers the first semiconductor layer;

[0084] S11. Form a first electrode on the portion of the conductive film layer extending into the first opening region, and form a second electrode on the portion of the conductive film layer extending into the second opening region.

[0085] It should be noted that in S8, laser or mask etching is used to etch an opening on the second semiconductor layer on the back of the silicon wafer to form a second opening area, and the second semiconductor layer in the second opening area is etched away. Laser etching is preferred, and the etching laser is an ultraviolet laser or a green laser with a pulse width of less than 50ns.

[0086] In S9, a conductive film layer is deposited on the back of the silicon wafer using physical vapor deposition (PVD) or activated plasma deposition (RPD).

[0087] In S10, an isolation groove is formed on the conductive film layer by laser or etching.

[0088] In S11, the silver gate electrode can be formed by screen printing and low temperature sintering, or the gate line electrode can be formed by electroplating. Preferably, the gate line electrode is formed by electroplating (the first electrode and the second electrode are both formed by electroplating).

[0089] In a third aspect, the present invention provides a photovoltaic module, which includes the above-mentioned high short-circuit current back contact cell.

[0090] The embodiments of the present invention are described in detail below, which are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.

[0091] Example 1

[0092] A back contact battery is prepared by the following steps:

[0093] S1. Figure 1 As shown, the back side of an N-type single crystal silicon wafer 1 is polished and cleaned, and the silicon wafer 1 is a Czochralski single crystal silicon wafer.

[0094] S2. Figure 2 As shown, a first semiconductor layer and a mask layer 4 are sequentially formed on the back of the silicon wafer 1, and the first semiconductor layer includes a tunneling oxide layer 2 and a first doping layer 3. Both the first semiconductor layer and the mask layer 4 are deposited by in-situ doping using tubular PECVD. In the first stage, 9000sccm of laughing gas is introduced, and the tunneling oxide layer 2 is formed by chemical reaction under the condition of turning on the glow. The reaction conditions of the first stage are: reaction temperature of 400°C, reaction pressure of 1000mtorr, reaction time of 30s, and thickness of the tunneling oxide layer 2 is 1.5nm; in the second stage, 2000sccm of silane, 2000sccm of phosphine and hydrogen (phosphine to hydrogen flow ratio of 98:2) are introduced, and the carbon-doped first doping layer 3 is formed by chemical reaction under the condition of turning on the glow. The reaction conditions of the second stage are: reaction temperature of 400°C, reaction time of 1000s, reaction pressure of 1000mtorr, thickness of the first doping layer 3 is 150nm, and carbon doping concentration is 1e19cm -3 The mask layer 4 is made of silicon nitride and has a thickness of 80 nm.

[0095] S3. Figure 2As shown, nitrogen gas is introduced to anneal the first semiconductor layer, and the annealing conditions are: annealing pressure of 250 mbar, annealing temperature of 900° C., nitrogen flow rate of 5000 sccm, and annealing time of 30 min.

[0096] S4. Figure 3 As shown, a laser is used to etch an opening on the back of the silicon wafer 1 to form a first opening area. The width S102 of the first opening area is 0.3 mm, and the mask layer 4 and the first semiconductor layer in the first opening area are etched away. The laser is an ultraviolet laser with a pulse width of 50ns.

[0097] S5. Figure 3 As shown, the mask layer 4 and the first semiconductor layer remaining in the first opening area are removed by texturing and cleaning, and a velvet surface is formed on the front side of the silicon wafer 1 and in the first opening area. Then, the mask layer 4 outside the first opening area on the back side of the silicon wafer 1 is removed by hydrofluoric acid cleaning.

[0098] S6. Figure 4 As shown, an oxide layer 5 and an anti-reflection layer 7 are sequentially formed on the front side of the silicon wafer 1. The anti-reflection layer 7 is silicon nitride. The formation process is as follows:

[0099] In the first stage, laughing gas is introduced and oxidized under the condition of turning on the glow to form an oxide layer 5, the thickness of the oxide layer 5 is 5nm, and the reaction conditions of the first stage are: reaction temperature is 400°C, laughing gas flow rate is 6000sccm, reaction pressure is 2000mtorr, reaction time is 300s, and reaction power is 5kW;

[0100] In the second stage, a mixed gas of 2% phosphine and 98% hydrogen is introduced, and the oxide layer 5 is doped with phosphorus and hydrogen under the condition of turning on the glow to form a phosphorus-doped and hydrogen-doped region 6 on the oxide layer 5. The depth of the phosphorus-doped and hydrogen-doped region 6 is 2.5 nm. The reaction conditions of the second stage are: reaction temperature of 400°C, phosphine flow rate of 400 sccm, reaction pressure of 200 mtorr, reaction time of 200 s, reaction power of 2 kW, and phosphorus doping concentration of 3e18 cm -3 , the hydrogen atomic content is 6e18cm -3 ;

[0101] In the third stage, silane and ammonia are introduced, and an anti-reflection layer 7 is formed under the condition of turning on the glow. The thickness of the anti-reflection layer 7 is 100 nm and the refractive index is 2.3. The reaction conditions of the third stage are: reaction temperature is 400°C, silane flow rate is 1400sccm, ammonia flow rate is 6000sccm, reaction pressure is 2000mtorr, reaction time is 800s, and reaction power is 5kW.

[0102] S7. Figure 5As shown, a second semiconductor layer is deposited on the back of the silicon wafer 1 by plasma enhanced chemical vapor deposition (PECVD) technology, and the second semiconductor layer includes an intrinsic amorphous silicon layer 8 and a second doping layer 9. The thickness of the intrinsic amorphous silicon layer 8 is 10 nm, the thickness of the second doping layer 9 is 20 nm, and the boron doping concentration in the second doping layer 9 is 1e19 cm -3 .

[0103] S8. Figure 5 As shown, a laser is used to etch an opening on the back of the silicon wafer 1 to form a second opening area that is alternately arranged with the first opening area and spaced apart. The width S101 of the second opening area is 0.2 mm, and the second semiconductor layer in the second opening area is etched away. The laser is an ultraviolet laser with a pulse width of 20 ns.

[0104] S9. Figure 6 As shown, a transparent conductive film layer 10 is deposited on the back of a silicon wafer 1 by physical vapor deposition (PVD) technology. The thickness of the conductive film layer 10 is 60 nm, and the material of the conductive film layer 10 is a tin oxide-doped indium oxide thin film.

[0105] S10. Figure 6 As shown, an isolation groove is formed on the conductive film layer 10 by laser, the isolation groove is located between the second opening area and the first opening area, and the width of the isolation groove is 80 μm;

[0106] S11. Figure 7 As shown, a first electrode is formed on a portion of the conductive film layer 10 extending into the first opening region, and a second electrode is formed on a portion of the conductive film layer 10 extending into the second opening region by electroplating.

[0107] Example 2

[0108] The method of Example 1 is referred to, except that the depth of the phosphorus-doped and hydrogen-doped region 6 formed on the oxide layer 5 is adjusted to 3 nm.

[0109] Example 3

[0110] The method of Example 1 is followed, except that the phosphorus doping concentration in the phosphorus-doped and hydrogen-doped region 6 is adjusted to 1e18 cm -3 , the hydrogen content is 5e18cm -3 .

[0111] Example 4

[0112] The method of Example 1 is referred to, except that the thickness of the oxide layer 5 is adjusted to 4 nm.

[0113] Example 5

[0114] The method of Example 1 is followed, except that the carbon doping concentration in the first doping layer 3 is adjusted to 8e19cm -3 , and the boron doping concentration in the second doping layer 9 is adjusted to 4e20cm -3 .

[0115] Comparative Example 1

[0116] The method of Example 1 is referred to, except that the structure of the front side of the silicon wafer 1 is different. On the front side of the silicon wafer 1, an intrinsic amorphous hydrogenated silicon with a thickness of 5 nm, a phosphorus-doped hydrogenated amorphous silicon with a thickness of 10 nm, and an anti-reflection layer 7 with a thickness of 100 nm are sequentially formed.

[0117] Comparative Example 2

[0118] The method of Example 1 is referred to, except that the depth of the phosphorus-doped and hydrogen-doped region 6 formed on the oxide layer 5 is adjusted to 0.5 nm.

[0119] Comparative Example 3

[0120] The method of Example 1 is followed, except that the phosphorus doping concentration in the phosphorus-doped and hydrogen-doped region 6 is adjusted to 1e17 cm -3 .

[0121] Comparative Example 4

[0122] The method of Example 1 is followed, except that the hydrogen atom content in the phosphorus-doped and hydrogen-doped region 6 is adjusted to 1e17 cm -3 .

[0123] Comparative Example 5

[0124] The method of Example 1 is referred to, except that the reaction conditions of the second stage of S6 are adjusted as follows: reaction temperature is 500° C., phosphine flow rate is 600 sccm, reaction pressure is 400 mtorr, reaction time is 300 s, and reaction power is 4 kW.

[0125] Test Case

[0126] The back contact cells obtained in the above examples and comparative examples were subjected to performance tests, and the results are shown in Table 1.

[0127] Table 1

[0128]

[0129] It can be seen from the above results that, compared with the comparative example, the embodiment of the present invention can provide a field passivation effect through the phosphorus-doped and hydrogen-doped region 6 on the oxide layer 5, effectively passivate surface defects, improve the passivation level, and enable the back-contact battery to maintain a higher open-circuit voltage. In addition, the N-type polysilicon layer / N-type amorphous silicon layer is eliminated, which can reduce optical losses to a minimum, so that the back-contact battery has a higher short-circuit current.

[0130] Furthermore, according to Example 1 and Examples 2-5, it can be seen that the preferred battery structure of the present invention is more conducive to maintaining a high open circuit voltage while having a higher short-circuit current, thereby improving the battery conversion efficiency.

[0131] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A back contact battery with high short-circuit current, characterized in that: The invention comprises a silicon wafer, an oxide layer and an anti-reflection layer arranged in sequence on the front side of the silicon wafer, wherein a phosphorus-doped and hydrogen-doped region is arranged on one side of the oxide layer close to the anti-reflection layer, wherein the depth of the phosphorus-doped and hydrogen-doped region is 1.6nm-3nm, and the phosphorus doping concentration is 1e18cm -3 -5e18cm -3 , the hydrogen content is 5e18cm -3 -8e18cm -3 ; The high short-circuit current back-contact battery further includes a first semiconductor layer and a second semiconductor layer disposed simultaneously on the back side of the silicon wafer, the first semiconductor layer being provided with a first opening region, a portion of the second semiconductor layer covering a side of the first semiconductor layer away from the silicon wafer, and another portion of the second semiconductor layer extending into the first opening region and covering the silicon wafer; The high short-circuit current back contact battery further comprises a conductive film layer, the conductive film layer is arranged on a side of the first semiconductor layer and the second semiconductor layer away from the silicon wafer, the second semiconductor layer is provided with a second opening area, the second opening area and the first opening area are alternately and spaced apart, a part of the conductive film layer extends into the first opening area and covers the second semiconductor layer, another part extends into the second opening area and covers the first semiconductor layer, and an isolation groove is provided between two adjacent parts of the conductive film layer; The high short-circuit current back-contact battery also includes a first electrode and a second electrode. The first electrode is arranged on the portion of the conductive film layer extending into the first opening area, and the second electrode is arranged on the portion of the conductive film layer extending into the second opening area.

2. The high short-circuit current back contact battery according to claim 1, characterized in that: The thickness of the oxide layer is 4nm-6nm; and / or the thickness of the anti-reflection layer is 80nm-110nm.

3. The high short-circuit current back contact battery according to claim 1 or 2, characterized in that: The anti-reflection layer is selected from at least one of silicon nitride, silicon oxynitride and silicon oxide; and / or the refractive index of the anti-reflection layer is 2.2-2.

5.

4. The high short-circuit current back contact battery according to claim 1, characterized in that: The first semiconductor layer includes a tunneling silicon oxide layer and a first doping layer, wherein the first doping layer is arranged on a side of the tunneling silicon oxide layer away from the silicon wafer, the thickness of the tunneling silicon oxide layer is 1nm-2nm, the thickness of the first doping layer is 150nm-300nm, and the phosphorus doping concentration in the first doping layer is 1e20cm -3 -5e20cm -3 The carbon doping concentration in the first doping layer is 1e19cm -3 -8e19cm -3 .

5. The high short-circuit current back contact battery according to claim 1, characterized in that: The second semiconductor layer includes an intrinsic amorphous silicon layer and a second doped layer, the second doped layer is arranged on a side of the intrinsic amorphous silicon layer away from the silicon wafer, the thickness of the intrinsic amorphous silicon layer is 5nm-15nm, the thickness of the second doped layer is 10nm-35nm, and the boron doping concentration in the second doped layer is 1e19cm -3 -4e20cm -3 .

6. A method for preparing a back contact battery with high short-circuit current, characterized in that: For preparing a back contact battery with a high short-circuit current as claimed in any one of claims 1 to 5, the method for preparing the back contact battery with a high short-circuit current comprises the following steps: S1. Polishing and cleaning the back side of the silicon wafer; S2. sequentially forming a first semiconductor layer and a mask layer on the back side of the silicon wafer; S3. Annealing the first semiconductor layer; S4. Etching an opening on the first semiconductor layer and the mask layer to form a first opening region; S5. Removing the first semiconductor layer and the mask layer remaining in the first opening region by texturing and cleaning, and forming a texture surface on the front side of the silicon wafer and in the first opening region; thereafter, cleaning and removing the mask layer outside the first opening region; S6. forming an oxide layer and an anti-reflection layer in sequence on the front side of the silicon wafer; wherein, firstly, introducing nitrous oxide and oxidizing the oxide layer under the condition of turning on the glow to form the oxide layer; then introducing a mixed gas of 2% phosphine and 98% hydrogen, and performing phosphorus-doped and hydrogen-doped treatment on the oxide layer under the condition of turning on the glow to form a phosphorus-doped and hydrogen-doped region on the oxide layer; then introducing silane and ammonia, and forming the anti-reflection layer under the condition of turning on the glow; S7. Form a second semiconductor layer on the back side of the silicon wafer, so that a portion of the second semiconductor layer covers the side of the first semiconductor layer away from the silicon wafer, and another portion extends into the first opening area and covers the silicon wafer.

7. The method for preparing a back contact battery with high short-circuit current according to claim 6, characterized in that: In S6, the reaction conditions for forming the oxide layer are: reaction temperature of 400° C.-450° C., nitrous oxide flow rate of 5000 sccm-8000 sccm, reaction pressure of 1000 mtorr-3000 mtorr, reaction time of 240 s-360 s, and reaction power of 4 kW-6 kW; and / or, the reaction conditions for forming the phosphorus-doped and hydrogen-doped regions are: reaction temperature of 400° C.-450° C., phosphine flow rate of 300 sccm-500 sccm, reaction pressure of 100 mtorr-300 mtorr, reaction time of 120 s-240 s, and reaction power of 1.5 kW-3 kW; And / or, the reaction conditions for forming the anti-reflection layer are: reaction temperature of 400°C-450°C, silane flow rate of 1200sccm-1600sccm, ammonia flow rate of 5000sccm-8000sccm, reaction pressure of 500mtorr-3000mtorr, reaction time of 700s-1000s, and reaction power of 4kW-6kW.

8. The method for preparing a back contact battery with high short-circuit current according to claim 6, characterized in that: After S7, the method for preparing the high short-circuit current back contact battery further includes: S8. Etching openings on the second semiconductor layer to form second opening regions alternately arranged with the first opening regions and spaced apart, followed by cleaning; S9. Forming a conductive film layer on the back side of the silicon wafer; S10. An isolation groove is formed on the conductive film layer so that a portion of the conductive film layer separated from each other extends into the first opening area and covers the second semiconductor layer, and another portion extends into the second opening area and covers the first semiconductor layer; S11. Form a first electrode on the portion of the conductive film layer extending into the first opening region, and form a second electrode on the portion of the conductive film layer extending into the second opening region.

9. A photovoltaic module, characterized in that: A back contact battery with high short-circuit current comprising the battery as claimed in any one of claims 1 to 5.

Citation Information

Patent Citations

  • Back contact solar cell, preparation method and cell module

    CN115188837A

  • Short-process preparation method of combined passivation back contact battery and application of short-process preparation method

    CN117133834A

  • Back contact battery with specific front passivation structure and preparation method and application thereof

    CN117577697A

  • Combined passivation back contact cell based on P-type silicon wafer, preparation thereof and photovoltaic module

    CN117577708A

  • Preparation method of back contact solar cell, solar cell and cell module

    CN117954509A