In-situ growth of MOF-derived Co / MnO on nickel foam x Doped oxide catalysts, their preparation methods and applications

By growing Co/MnOx doped oxide catalysts derived from CoMn-MOF-74 in situ on nickel foam, the problems of high oxidation conversion temperature and complex preparation of existing foam metal catalysts are solved, achieving low-temperature and high-efficiency catalytic oxidation of CO, which is suitable for applications such as room temperature purification and high-purity oxygen production.

CN118513048BActive Publication Date: 2026-11-17CHANGZHOU UNIV
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410561204.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-08
Publication Date
2026-11-17
Estimated Expiration
2044-05-08

AI Technical Summary

Technical Problem

When existing foam metal catalysts are used to remove CO, the oxidation conversion temperature is high, the catalyst preparation process is complex and costly, and the small specific surface area leads to insufficient adsorption of reactant molecules and exposure of active sites.

Method used

Co/MnOx doped oxide catalysts derived from CoMn-MOF-74 were grown in situ on nickel foam. CoMn-MOF-74 was grown in situ on nickel foam and then calcined in an air atmosphere to form Co/MnOx doped oxides, forming a multi-level hierarchical structure to improve the specific surface area.

Benefits of technology

It achieves efficient catalytic oxidation of CO over a wide temperature range (25 °C to 800 °C), especially maintaining 100% conversion rate at low temperatures and maintaining stable conversion rate for 20 h at room temperature. It is suitable for room temperature purification, pure oxygen production, and CO oxidation in hydrocarbon fuel combustion products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

This invention discloses an in-situ growth method for MOF-derived Co / MnO on nickel foam. x This invention relates to doped oxide catalysts, their preparation methods, and applications, belonging to the field of catalytic oxidation for CO removal. The invention first involves in-situ growth of CoMn-MOF-74 on nickel foam, followed by high-temperature calcination to obtain MOF-derived Co / MnO. x Doped oxide catalyst. This invention utilizes non-precious metal doping, high temperature, nanoengineering, and interface technology to achieve low-temperature vaporization of carbonates on the catalyst surface, releasing active sites and achieving 100% conversion of CO to CO2 at 25-800℃, and 90% conversion to CO2 even at a low temperature of 8℃.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of catalytic oxidation for CO removal, specifically relating to a method for in-situ growth of MOF-derived Co / MnO on nickel foam. x Novel catalysts doped with oxides, their preparation methods, and applications. Background Technology

[0002] CO, as one of the major air pollutants, readily binds to hemoglobin in the human body, leading to tissue hypoxia and even suffocation. When the concentration of CO in the air reaches 650 ppm, males will experience poisoning symptoms within one hour. Furthermore, in the petrochemical industry, many catalysts used in chemical processes are highly sensitive to CO; even trace amounts can poison or deactivate them. Therefore, the effective elimination of CO remains a problem to be solved in many aspects of industrial production.

[0003] Currently, catalytic oxidation of CO is one of the most common and effective methods for eliminating CO. CO oxidation catalysts can be divided into two main categories: noble metal catalysts and non-metallic catalysts.

[0004] Chinese patent CN107519871A uses AuAg alloy particles with SiO2 as the outer shell to prepare AuAg@SiO2 nanocatalysts for the catalytic oxidation of CO, which can completely convert CO to CO2 at 70℃. Chinese patent CN113117693A provides a Pd-Cu / TiO2 bimetallic catalyst for the catalytic oxidation of CO, with a catalytic temperature of 20-120℃. Chinese patent CN110876943A uses an oxide-modified PtCo bimetallic catalyst for CO oxidation, achieving a LaCo oxidation at 380℃. 0 .99 Pt 0 .01 The O3-catalyzed CO conversion rate is 100%. Chinese patent CN111659382A describes the preparation of rod-shaped γ-Al2O3 via a hydrothermal method, followed by the preparation of an Au-supported catalyst, Au / Al2O3, using an equal-volume impregnation method. The catalyst's catalytic performance was evaluated using the CO oxidation reaction, and it maintained good oxidation performance even after high-temperature calcination at 700 °C.

[0005] While precious metals exhibit excellent performance in the catalytic oxidation of CO, their scarcity and high price make them unsuitable for large-scale applications. Given the challenges of applying precious metal catalysts in practical industrial applications, some variable-valence transition metal oxides, which generate oxygen vacancies and defects during valence state changes to promote the reaction, have become a research hotspot in recent years due to their abundant reserves and low cost. Chinese patent CN1554480A describes a CuO / CeO2 catalyst prepared using a combination of sol-gel and impregnation methods, with a CuO mass ratio ranging from 3.78% to 15.12%, achieving 100% CO conversion above 140 °C.

[0006] However, most transition metal catalysts exist in powder form, making them unsuitable for industrial applications, primarily due to high pressure drops. Furthermore, powdered catalysts exposed to industrial processes are easily washed away, resulting in catalyst loss and increasing the risk of secondary contamination. A common approach to overcoming these drawbacks is to load powdered materials onto monolithic substrates; porous structures are essential for these substrates to meet the requirements of low pressure drops and high surface-to-volume ratios in practical applications. In recent years, metal foams have been used as catalyst supports due to their well-designed three-dimensional channels, unique mechanical plasticity, and excellent thermal conductivity.

[0007] Chinese patent CN1593756A uses a nickel-chromium stainless steel honeycomb (referred to as a metal honeycomb carrier) as the first carrier and activated alumina powder as the second carrier. Small amounts of rare earth element oxides such as CeO2, La2O3, ZrO2, and Y2O3 are added as promoters and stabilizers. The active component is mainly PtO2 or PdO, or a combination of both, to prepare a metal honeycomb carrier catalyst. The coating of the metal honeycomb carrier catalyst prepared by this method is not easily peeled off, has good ignition performance, and exhibits high activity as a three-way catalyst, capable of simultaneously purifying CO, HC, and NO in exhaust gas. x It has a wide operable window. Chinese patent CN110975610A uses a conventional aluminum honeycomb structure as a carrier and employs a catalyst slurry prepared by mixing and homogenizing deionized water, organic manganese salt, organic nickel salt, alumina powder, boehmite, and a film-forming agent. The slurry is then sprayed, purged, dried, and calcined to obtain the finished product. This room-temperature ozone decomposition honeycomb module features lightweight, corrosion resistance, low wind resistance, high decomposition efficiency, and long service life. The module preparation process is simple and environmentally friendly, producing no gaseous pollutants such as nitrogen oxides and sulfur oxides, nor any wastewater discharge. The resulting honeycomb module can be applied to the catalytic decomposition and treatment of ozone in the air. Under conditions of 10-40 ℃ and 30-98 RH%, the ozone concentration is 1-20 mg / m³. 3 All can be effectively degraded to 0.02 mg / m³ 3The ozone degradation rate exceeds 98%, achieving the purification requirement of effective ozone removal for a long time (>3500 h). Chinese patent CN108615610A provides a cobalt-manganese bimetallic hydroxide composite material grown in situ on a nickel foam substrate. This composite material can be used as an ideal supercapacitor and a high-performance electrocatalytic material.

[0008] There is limited research on the use of foamed metal catalysts for CO removal in current technologies. CO oxidation involves high conversion temperatures, complex catalyst preparation processes, and high costs. This may be related to the small specific surface area of ​​foamed metal catalysts, which hinders the adsorption of reactant molecules, the exposure of active sites, and the generation of surface defects. Summary of the Invention

[0009] This invention aims to provide a method for in-situ growth of Co / MnO derived from CoMn-MOF-74 on nickel foam. X Novel oxide-doped catalysts, their preparation methods, and applications are described. These catalysts exhibit a wide applicable temperature range and excellent stability, and can achieve efficient catalytic oxidation even at low temperatures.

[0010] This invention first provides a method for preparing Co / MnOx doped oxides derived from CoMn-MOF-74 by in-situ growth on nickel foam, specifically including the following steps: S1. CoMn-MOF-74 is grown in situ on nickel foam to obtain CoMn-MOF-74 / NF; wherein the molar ratio of Co to Mn is 0.3-3:1. Specifically, cobalt source, manganese source, and 2,5-dihydroxyterephthalic acid are dissolved in a mixed solvent of dimethylformamide / ethanol / water, nickel foam is added, and the mixture is transferred to a reaction vessel for reaction. After the reaction is completed, the mixture is centrifuged, washed, and dried to obtain flake-shaped CoMn-MOF-74 / NF.

[0011] The molar ratio of cobalt source, manganese source, and 2,5-dihydroxyterephthalic acid is 1-3:1-3:1.5.

[0012] The cobalt source is cobalt salts such as cobalt nitrate and cobalt acetate, or their hydrates; the manganese source is manganese salts such as manganese nitrate and manganese acetate, or their hydrates. In the mixed solvent of dimethylformamide / ethanol / water, the volume ratio of dimethylformamide (DMF), anhydrous ethanol and water is 15:1:1.

[0013] The reaction temperature is 130-180℃, and the reaction time is 20-24 h.

[0014] Nickel foam was obtained by ultrasonically cleaning with deionized water, hydrochloric acid (3 mg / L), and anhydrous ethanol for 10 min, and then drying in a vacuum drying oven at 60℃ for 12 h.

[0015] S2. Calcine CoMn-MOF-74 / NF in air atmosphere to obtain Co / MnO. x Oxide-supported nickel foam catalyst Co / Mn3O4-NF.

[0016] Specifically, CoMn-MOF-74 / NF is placed in a muffle furnace and calcined in an air atmosphere.

[0017] The calcination temperature is 200-400 ℃; preferably 300 ℃.

[0018] The calcination time is 2-4 hours; preferably 3 hours. The heating rate is 1-10 ℃ / min; preferably 1 ℃ / min.

[0019] Based on the above preparation method, this invention provides an in-situ growth of Co / MnO derived from CoMn-MOF-74 on nickel foam. X Catalysts doped with oxides, namely MOF-derived Co / MnO X Oxide-supported nickel foam catalyst.

[0020] The Co / MnO prepared by this invention x -NF catalysts show that a number of one-dimensional short rod-shaped structures are loaded on the surface of nickel foam. These short rod-shaped structures are composed of stacked two-dimensional sheet-like structures with multi-layer morphology. This multi-level layered structure may effectively improve the specific surface area.

[0021] This invention also provides in-situ growth of Co / MnO derived from CoMn-MOF-74 on the aforementioned nickel foam. x The application of doped oxide catalysts in CO conversion, especially in the following three aspects: (1) Purification of CO-containing air at room temperature (25 ℃) or below zero. CO is produced by the combustion of hydrocarbons. By catalytically oxidizing the gas in the indoor space, the toxic and harmful CO is converted into non-toxic and harmless CO2.

[0022] (2) Preparation of high-purity oxygen. Pure oxygen contains trace amounts of CO, which is difficult to remove. The novel catalyst of Co-MnOx doped oxide grown in situ on nickel foam provided by this invention converts CO in oxygen into CO2, which is then adsorbed by CO2 adsorption materials, such as alumina, thereby achieving the removal of CO from oxygen and the preparation of high-purity oxygen.

[0023] (3) Oxidation of CO in the combustion products of hydrocarbon fuels (such as gasoline engines, diesel engines, etc.).

[0024] Compared with existing technologies, this invention uses CoMn-MOF-74 as a precursor and nickel foam as a support to prepare a nickel-based catalyst supported on a bimetallic oxide through high-temperature calcination. This catalyst achieves 100% CO conversion in the temperature range of 25 °C to 800 °C, and also achieves 90% CO2 conversion at 8 °C. Furthermore, the CO conversion rate remains at 100% for 20 hours at room temperature. The preparation method of this invention is simple, and the prepared catalyst has a wide temperature range for CO catalytic oxidation and exhibits good catalytic activity even at low temperatures, providing a research and development approach for low-temperature catalytic oxidation. Attached Figure Description

[0025] Figure 1 Co / MnO derived from CoMn-MOF-74 was grown in situ on nickel foam provided in Example 1. x Electron microscope image of a novel catalyst doped with oxides.

[0026] Figure 2 Co / MnO derived from CoMn-MOF-74 was grown in situ on nickel foam provided in Example 1. x Transmission electron microscope image of a novel catalyst doped with oxides.

[0027] Figure 3 Co / MnO derived from CoMn-MOF-74 was grown in situ on nickel foam provided in Example 1. x XRD pattern of a novel catalyst doped with oxides.

[0028] Figure 4 Co / MnO derived from CoMn-MOF-74 was grown in situ on nickel foam provided in Example 1. x A graph showing the relationship between CO conversion rate and reaction temperature for novel oxide-doped catalysts.

[0029] Figure 5 Co / MnO derived from CoMn-MOF-74 was grown in situ on nickel foam provided in Example 1. x Long-term CO oxidation at room temperature using a novel oxide-doped catalyst. Detailed Implementation

[0030] The present invention will be described in detail below with reference to the embodiments, but these should not be construed as limiting the scope of protection of the present invention. Example 1

[0031] The preparation method of this novel catalyst for in-situ growth of Co / MnOx doped oxides derived from CoMn-MOF-74 on nickel foam (NF) includes the following steps: 3 mmol of cobalt nitrate and 3 mmol of manganese nitrate are mixed with 1.5 mmol of 2,5-dihydroxyterephthalic acid, and approximately 60 ml of a mixed solvent of dimethylformamide, ethanol, and water in a volume ratio of 15:1:1 (52.5 ml:3.5 ml:3.5 ml) is added. After thorough stirring, 5 pieces of nickel foam (1 cm × 1 cm) are added, and then the mixture is transferred to a reaction vessel and kept at 130 °C for 24 h. The collected nickel foam is washed two to three times with DMF and methanol. It is then placed in an oven and dried at 80 °C for 12 h. The obtained sheet-like catalyst was placed in a muffle furnace and calcined in air at 300 °C for 3 h at a heating rate of 1 °C / min to obtain a novel catalyst (Co / Mn3O4-NF) of MOF-74-derived Co / MnOx doped oxide grown in situ on nickel foam. Example 2

[0032] The preparation method of this novel catalyst, which is derived from CoMn-MOF-74 and used to grow Co / MnOx doped oxides in situ on nickel foam, includes the following steps: 3 mmol of cobalt nitrate and 1 mmol of manganese nitrate are mixed with 1.5 mmol of 2,5-dihydroxyterephthalic acid, and a mixture of dimethylformamide, ethanol, and water in a volume ratio of 15:1:1 (52.5 ml:3.5 ml:3.5 ml) is added to a final volume of 60 ml. After thorough stirring, 5 pieces of nickel foam (1 cm × 1 cm) are added, and the mixture is then transferred to a reaction vessel and kept at 130 °C for 24 h. The collected nickel foam is washed two to three times with DMF and methanol. It is then placed in an oven and dried at 80 °C for 12 h. The obtained sheet-like catalyst was placed in a muffle furnace and calcined in air at 300 °C for 3 h at a heating rate of 1 °C / min to obtain a novel catalyst (Co3Mn1-NF) of Co / MnOx doped oxide derived from MnCo-MOF-74 grown in situ on nickel foam. Example 3

[0033] The preparation method of this novel catalyst, which is derived from CoMn-MOF-74 and used to grow Co / MnOx doped oxides in situ on nickel foam, includes the following steps: 1 mmol of cobalt nitrate and 3 mmol of manganese nitrate are mixed with 1.5 mmol of 2,5-dihydroxyterephthalic acid, and a mixture of dimethylformamide, ethanol, and water in a volume ratio of 15:1:1 (52.5 ml:3.5 ml:3.5 ml) is added to a final volume of 60 ml. After thorough stirring, 5 pieces of nickel foam (1 cm × 1 cm) are added, and the mixture is then transferred to a reaction vessel and kept at 130 °C for 24 h. The collected nickel foam is washed two to three times with DMF and methanol. It is then placed in an oven and dried at 80 °C for 12 h. The obtained sheet-like catalyst was placed in a muffle furnace and calcined in air at 300 °C for 3 h at a heating rate of 1 °C / min to obtain a novel catalyst (Co1Mn3-NF) of Co / MnOx doped oxide derived from MnCo-MOF-74 grown in situ on nickel foam. Example 4

[0034] The preparation method of this novel catalyst for in-situ growth of Co / MnOx doped oxides derived from CoMn-ZIF-67 on nickel foam includes the following steps: 1 mmol of cobalt nitrate and 3 mmol of manganese nitrate are mixed with 1.5 mmol of dimethylimidazole, and a mixture of dimethylformamide, ethanol, and water in a volume ratio of 15:1:1 (52.5 ml:3.5 ml:3.5 ml) is added to a final volume of 60 ml. After thorough stirring, 5 pieces of nickel foam (1 cm × 1 cm) are added and kept at 25 °C for 24 h. The mixture is washed two to three times with water and methanol. Then, it is placed in an oven and dried at 80 °C for 12 h. The resulting sheet-like catalyst is placed in a muffle furnace and calcined in air at 300 °C for 3 h at a heating rate of 1 °C / min to obtain a novel catalyst (Co / Mn3O4-NF-ZIF-67) for in-situ growth of Co / MnOx doped oxides derived from MnCo-MOF on nickel foam. Example 5

[0035] The preparation method of this novel catalyst for in-situ growth of Co / MnOx doped oxides derived from CoMn-MOF on nickel foam includes the following steps: 1 mmol of cobalt nitrate and 3 mmol of manganese nitrate are mixed with 1.5 mmol of terephthalic acid, and a mixture of dimethylformamide, ethanol, and water in a volume ratio of 15:1:1 (52.5 ml:3.5 ml:3.5 ml) is added to a final volume of 60 ml. After thorough stirring, 5 pieces of nickel foam (1 cm × 1 cm) are added, and then the mixture is transferred to a reaction vessel and kept at 130 °C for 24 h. The collected nickel foam is washed two to three times with DMF and methanol. It is then placed in an oven and dried at 80 °C for 12 h. The resulting sheet-like catalyst is placed in a muffle furnace and calcined in air at 300 °C for 3 h at a heating rate of 1 °C / min to obtain a novel catalyst (Co / Mn3O4-NF-BDC) for in-situ growth of Co / MnOx doped oxides derived from MnCo-MOF on nickel foam. Example 6

[0036] The preparation method of this novel catalyst for in-situ growth of Mn-MOF-74-derived Co / MnOx doped oxides on nickel foam includes the following steps: 3 mmol of cobalt nitrate and 3 mmol of manganese nitrate are mixed with 1.5 mmol of 2,5-dihydroxyterephthalic acid, and a mixture of dimethylformamide, ethanol, and water in a volume ratio of 15:1:1 (52.5 ml:3.5 ml:3.5 ml) is added to a final volume of 60 ml. After thorough stirring, 5 pieces of nickel foam (1 cm × 1 cm) are added, and then the mixture is transferred to a reaction vessel and kept at 130 °C for 24 h. The collected nickel foam is washed two to three times with DMF and methanol. It is then placed in an oven and dried at 80 °C for 12 h. The obtained sheet-like catalyst was placed in a muffle furnace and calcined in air at 200 °C for 3 h at a heating rate of 1 °C / min to obtain a novel catalyst (Co / Mn3O4-NF-200) of MOF-74-derived Co / MnOx doped oxide grown in situ on nickel foam. Example 7

[0037] The preparation method of this novel catalyst for in-situ growth of Mn-MOF-74-derived Co / MnOx doped oxides on nickel foam includes the following steps: 3 mmol of cobalt nitrate and 3 mmol of manganese nitrate are mixed with 1.5 mmol of 2,5-dihydroxyterephthalic acid, and a mixture of dimethylformamide, ethanol, and water in a volume ratio of 15:1:1 (52.5 ml:3.5 ml:3.5 ml) is added to a final volume of 60 ml. After thorough stirring, 5 pieces of nickel foam (1 cm × 1 cm) are added, and then the mixture is transferred to a reaction vessel and kept at 130 °C for 24 h. The collected nickel foam is washed two to three times with DMF and methanol. It is then placed in an oven and dried at 80 °C for 12 h. The obtained sheet-like catalyst was placed in a muffle furnace and calcined in air at 400 °C for 3 h at a heating rate of 1 °C / min to obtain a novel catalyst (Co / Mn3O4-NF-400) of MOF-74-derived Co / MnOx doped oxide grown in situ on nickel foam. Example 8

[0038] The preparation method of this novel catalyst for in-situ growth of Mn-MOF-74-derived Co-MnOx doped oxide on nickel foam includes the following steps: 3 mmol of cobalt nitrate and 3 mmol of manganese nitrate are mixed with 1.5 mmol of 2,5-dihydroxyterephthalic acid, and a mixture of dimethylformamide, ethanol, and water in a volume ratio of 15:1:1 (52.5 ml:3.5 ml:3.5 ml) is added to a final volume of 60 ml. After thorough stirring, 5 pieces of nickel foam (1 cm × 1 cm) are added, and then the mixture is transferred to a reaction vessel and kept at 130 °C for 24 h. The collected nickel foam is washed two to three times with DMF and methanol. It is then placed in an oven and dried at 80 °C for 12 h. The obtained sheet-like catalyst was placed in a muffle furnace and calcined in air at 400 °C for 2 h at a heating rate of 1 °C / min to obtain a novel catalyst (Co / Mn3O4-NF-2) of MOF-74-derived Co / MnOx doped oxide grown in situ on nickel foam. Example 9

[0039] The preparation method of this novel catalyst for in-situ growth of Mn-MOF-74-derived Co-MnOx doped oxide on nickel foam includes the following steps: 3 mmol of cobalt nitrate and 3 mmol of manganese nitrate are mixed with 1.5 mmol of 2,5-dihydroxyterephthalic acid, and a mixture of dimethylformamide, ethanol, and water in a volume ratio of 15:1:1 (52.5 ml:3.5 ml:3.5 ml) is added to a final volume of 60 ml. After thorough stirring, 5 pieces of nickel foam (1 cm × 1 cm) are added, and then the mixture is transferred to a reaction vessel and kept at 130 °C for 24 h. The collected nickel foam is washed two to three times with DMF and methanol. It is then placed in an oven and dried at 80 °C for 12 h. The obtained sheet-like catalyst was placed in a muffle furnace and calcined in air at 400 °C for 4 h at a heating rate of 1 °C / min to obtain a novel catalyst (Co / Mn3O4-NF-4) of MOF-74-derived Co / MnOx doped oxide grown in situ on nickel foam. Example 10

[0040] The preparation method of this novel catalyst for in-situ growth of Mn-MOF-74-derived Co / MnOx doped oxides on nickel foam includes the following steps: 3 mmol of cobalt nitrate and 3 mmol of manganese nitrate are mixed with 1.5 mmol of 2,5-dihydroxyterephthalic acid, and a mixture of dimethylformamide, ethanol, and water in a volume ratio of 15:1:1 (52.5 ml:3.5 ml:3.5 ml) is added to a final volume of 60 ml. After thorough stirring, 5 pieces of nickel foam (1 cm × 1 cm) are added, and then the mixture is transferred to a reaction vessel and kept at 130 °C for 24 h. The collected nickel foam is washed two to three times with DMF and methanol. It is then placed in an oven and dried at 80 °C for 12 h. The obtained sheet-like catalyst was placed in a muffle furnace and calcined in air at 400 °C for 3 h at a heating rate of 5 °C / min to obtain a novel catalyst (Co / Mn3O4-NF-5) of MOF-74-derived Co / MnOx doped oxide grown in situ on nickel foam. Example 11

[0041] The preparation method of this novel catalyst for in-situ growth of Mn-MOF-74-derived Co / MnOx doped oxides on nickel foam includes the following steps: 3 mmol of cobalt nitrate and 3 mmol of manganese nitrate are mixed with 1.5 mmol of 2,5-dihydroxyterephthalic acid, and a mixture of dimethylformamide, ethanol, and water in a volume ratio of 15:1:1 (52.5 ml:3.5 ml:3.5 ml) is added to a final volume of 60 ml. After thorough stirring, 5 pieces of nickel foam (1 cm × 1 cm) are added, and then the mixture is transferred to a reaction vessel and kept at 130 °C for 24 h. The collected nickel foam is washed two to three times with DMF and methanol. It is then placed in an oven and dried at 80 °C for 12 h. The obtained sheet-like catalyst was placed in a muffle furnace and calcined in air at 400 °C for 3 h at a heating rate of 10 °C / min to obtain a novel catalyst (Co / Mn3O4-NF-10) of MOF-74-derived Co / MnOx doped oxide grown in situ on nickel foam. Example 12

[0042] The preparation method of this novel catalyst for in-situ growth of Mn-MOF-74-derived Co / MnOx doped oxides on nickel foam includes the following steps: 3 mmol of cobalt nitrate and 3 mmol of manganese nitrate are mixed with 1.5 mmol of 2,5-dihydroxyterephthalic acid, and a mixture of dimethylformamide, ethanol, and water in a volume ratio of 15:1:1 (52.5 ml:3.5 ml:3.5 ml) is added to a final volume of 60 ml. After thorough stirring, 5 pieces of nickel foam (1 cm × 1 cm) are added, and then the mixture is transferred to a reaction vessel and kept at 150 °C for 24 h. The collected nickel foam is washed two to three times with DMF and methanol. It is then placed in an oven and dried at 80 °C for 12 h. The obtained sheet-like catalyst was placed in a muffle furnace and calcined in air at 300 °C for 3 h at a heating rate of 1 °C / min to obtain a novel catalyst (Co / Mn3O4-NF-150) of MOF-74-derived Co / MnOx doped oxide grown in situ on nickel foam. Example 13

[0043] The preparation method of this novel catalyst for in-situ growth of Mn-MOF-74-derived Co / MnOx doped oxides on nickel foam includes the following steps: 3 mmol of cobalt nitrate and 3 mmol of manganese nitrate are mixed with 1.5 mmol of 2,5-dihydroxyterephthalic acid, and a mixture of dimethylformamide, ethanol, and water in a volume ratio of 15:1:1 (52.5 ml:3.5 ml:3.5 ml) is added to a final volume of 60 ml. After thorough stirring, 5 pieces of nickel foam (1 cm × 1 cm) are added, and then the mixture is transferred to a reaction vessel and kept at 180 °C for 24 h. The collected nickel foam is washed two to three times with DMF and methanol. It is then placed in an oven and dried at 80 °C for 12 h. The obtained sheet-like catalyst was placed in a muffle furnace and calcined in air at 300 °C for 3 h at a heating rate of 1 °C / min to obtain a novel catalyst (Co / Mn3O4-NF-180) of MOF-74-derived Co / MnOx doped oxide grown in situ on nickel foam. Example 14

[0044] The preparation method of this novel catalyst for in-situ growth of Mn-MOF-74-derived Co / MnOx doped oxides on nickel foam includes the following steps: 3 mmol of cobalt nitrate and 3 mmol of manganese nitrate are mixed with 1.5 mmol of 2,5-dihydroxyterephthalic acid, and a mixture of dimethylformamide, ethanol, and water in a volume ratio of 15:1:1 (52.5 ml:3.5 ml:3.5 ml) is added to a final volume of 60 ml. After thorough stirring, 5 pieces of nickel foam (1 cm × 1 cm) are added, and then the mixture is transferred to a reaction vessel and kept at 130 °C for 20 h. The collected nickel foam is washed two to three times with DMF and methanol. It is then placed in an oven and dried at 80 °C for 12 h. The obtained sheet-like catalyst was placed in a muffle furnace and calcined in air at 300 °C for 3 h at a heating rate of 1 °C / min to obtain a novel catalyst (Co / Mn3O4-NF-20) of MOF-74-derived Co / MnOx doped oxide grown in situ on nickel foam. Example 15

[0045] The preparation method of this novel catalyst for in-situ growth of Mn-MOF-74-derived Co / MnOx doped oxides on nickel foam includes the following steps: 3 mmol of cobalt nitrate and 3 mmol of manganese nitrate are mixed with 1.5 mmol of 2,5-dihydroxyterephthalic acid, and a mixture of dimethylformamide, ethanol, and water in a volume ratio of 15:1:1 (52.5 ml:3.5 ml:3.5 ml) is added to a final volume of 60 ml. After thorough stirring, 5 pieces of nickel foam (1 cm × 1 cm) are added, and the mixture is then transferred to a reaction vessel and kept at 130 °C for 22 h. The collected nickel foam is washed two to three times with DMF and methanol. It is then placed in an oven and dried at 80 °C for 12 h. The obtained sheet-like catalyst was placed in a muffle furnace and calcined in air at 300 °C for 3 h at a heating rate of 1 °C / min to obtain a novel catalyst (Co / Mn3O4-NF-22) of MOF-74-derived Co / MnOx doped oxide grown in situ on nickel foam.

[0046] The nickel foam (NF) used in the above examples was commercially available nickel foam that was ultrasonically cleaned for 10 min each with deionized water, hydrochloric acid (3 mg / L), and anhydrous ethanol. It was then dried in a vacuum drying oven at 60°C for 12 h to obtain the pretreated nickel foam.

[0047] The catalytic oxidation performance of a series of in-situ grown nickel foam oxides prepared in Examples 1-15 for CO oxidation was evaluated using a flow-through fixed-bed reactor. Reaction conditions: 1% CO, 10% O2, N2 balance gas, 5 catalyst flakes (1 cm × 1 cm), total flow rate of 100 mL / min, and space velocity per unit mass of 15000 mL / (g·h).

[0048] Table 1. Catalytic oxidation activity of various catalysts for CO removal (T) 90 (The temperature at which CO conversion reaches 90%)

[0049] The morphology and composition of the Co / Mn3O4-NF catalyst prepared in Example 1 were characterized.

[0050] 1. Images of the Co / Mn3O4-NF catalyst obtained using a scanning electron microscope are shown below. Figure 1Results Analysis: Numerous one-dimensional short rod-like structures were observed loaded on the surface of the nickel foam on the Co / Mn3O4-NF catalyst. These rod-like structures had a diameter of approximately 5 micrometers and a length of approximately 10-20 micrometers. These short rod-like structures exhibited good dispersion and no significant agglomeration. Furthermore, some of the short rods were composed of stacked two-dimensional sheet-like structures with multi-layered morphology. This multi-level layered structure may effectively increase the specific surface area of ​​the sample, which is beneficial for improving the sample's performance in adsorption and catalysis.

[0051] 2. Images of the Co / Mn3O4-NF catalyst obtained using transmission electron microscopy are shown below. Figure 2 Results analysis: The Co / Mn3O4-NF catalyst exhibits several lattice stripes with different spacings. Among them, the lattice stripe with a spacing of 0.466 nm corresponds to the (111) crystal plane of Co3O4, while the lattice stripe with a spacing of 0.288 nm can correspond to the (200) crystal plane of Mn3O4.

[0052] 3. XRD analysis of the Co / Mn3O4-NF catalyst is shown in [reference needed]. Figure 3 Results analysis: The Co / Mn3O4-NF catalyst exhibits characteristic peaks belonging to the (111), (200), and (220) crystal planes of Ni at 44.6°, 52.0°, and 76.4°, and characteristic peaks belonging to the (311) and (440) crystal planes of Co3O4 at 36.8° and 65.4°. The presence of a characteristic peak belonging to the (211) crystal plane of Mn3O4 at 36.2° indicates that the phase composition of this catalyst contains Mn3O4 and Co3O4 in addition to the Ni substrate.

[0053] The relationship between CO conversion rate and reaction temperature for Co / Mn3O4-NF, Co3O4-NF, Mn3O4-NF, and NF catalysts is shown in the figure. Figure 4 Results Analysis: From room temperature (25 ℃) to 800 ℃, the CO conversion rate of the Co / Mn3O4-NF catalyst was 100%. The CO conversion rates of both Co3O4-NF and Mn3O4-NF catalysts also reached 100% above 150 ℃. The CO conversion rate of the NF catalyst reached 100% above 400 ℃. Reaction conditions: 1% CO, 10% O2, N2 balance gas, 5 catalyst pieces (1 cm × 1 cm), total flow rate of 100 mL / min, and space velocity per unit mass of 15000 mL / (g·h).

[0054] The long-term CO oxidation results at 25 °C using the Co / Mn3O4-NF catalyst are shown in the figure. Figure 5Results analysis: The CO conversion rate of the Co / Mn3O4-NF catalyst remained at 100% within 20 h at 25 ℃. Reaction conditions: 1% CO, 10% O2, N2 balance gas, 5 catalyst pieces (1 cm × 1 cm), total flow rate of 100 mL / min, and space velocity per unit mass of 15000 mL / (g·h).

[0055] The novel catalyst provided by this invention, which utilizes Mn-MOF-74-derived Co / MnOx doped oxides grown in situ on nickel foam, efficiently oxidizes CO to CO2 within a temperature range of 5-800 °C under oxygen-containing conditions. Therefore, this invention provides an application of this novel catalyst in CO oxidation, particularly in the following three aspects: (1) Purification of CO-containing air at room temperature (25 ℃) or below zero. CO is produced by the combustion of hydrocarbons. By catalytically oxidizing the gas in the indoor space, the toxic and harmful CO is converted into non-toxic and harmless CO2.

[0056] (2) Preparation of high-purity oxygen. Pure oxygen contains trace amounts of CO, which is difficult to remove. The novel catalyst of Co / MnOx doped oxide grown in situ on nickel foam provided by this invention converts CO in oxygen into CO2, which is then adsorbed by CO2 adsorption materials, such as alumina, thereby achieving the removal of CO from oxygen and the preparation of high-purity oxygen.

[0057] (3) Oxidation of CO in the combustion products of hydrocarbon fuels (such as gasoline engines, diesel engines, etc.).

[0058] A novel catalyst, using Co / MnOx doped oxides grown in situ on nickel foam, achieves 100% CO conversion under various conditions. When the gas is anhydrous and the gas temperature ranges from 25 °C to 800 °C, 100% CO to CO2 conversion is achieved, with 80% conversion even at 8 °C. When the gas contains water, 100% CO to CO2 conversion is also achieved at temperatures between 150 °C and 800 °C. Furthermore, the CO conversion rate remains 100% at room temperature for 20 hours.

[0059] The above description is only a preferred embodiment of the present invention. It should be noted that for those skilled in the art, several improvements and modifications can be made without departing from the principle of the present invention, and these improvements and modifications should also be considered within the scope of protection of the present invention.

Claims

1. The application of a MOF-derived Co / MnOx doped oxide supported nickel foam catalyst, characterized in that, The preparation method of MOF-derived Co / MnOx doped oxide supported nickel foam catalyst includes the following specific steps: S1. Cobalt source, manganese source, and 2,5-dihydroxyterephthalic acid are dissolved in a mixed solvent of dimethylformamide / ethanol / water. Nickel foam is added, and the mixture is transferred to a reaction vessel for reaction. CoMn-MOF-74 is grown in situ on the nickel foam to obtain CoMn-MOF-74 / NF. The Co:Mn molar ratio is 1-3:

1. The reaction temperature is 130-180℃, and the reaction time is 20-24 h. S2. Calcine CoMn-MOF-74 / NF in air at a heating rate of 1-10 °C / min, a calcination temperature of 200-400 °C, and a calcination time of 2-4 h to obtain Co / MnO. x Doped oxide-supported nickel foam catalyst; The application is CO oxidation.

2. The application according to claim 1, characterized in that, The specific steps of step S1 also include: centrifugation, washing, and drying after the reaction is completed to obtain flake-shaped CoMn-MOF-74 / NF; the molar ratio of cobalt source, manganese source, and 2,5-dihydroxyterephthalic acid is 1-3:1:1.

5.

3. The application according to claim 1, characterized in that, The dimethylformamide / ethanol / water mixed solvent is prepared by mixing dimethylformamide, anhydrous ethanol and water in a volume ratio of 15:1:

1.

4. The application according to claim 1, characterized in that, The applications include the purification of CO-containing gases, the oxidation of CO in the preparation of high-purity oxygen, and the oxidation of CO produced by burning mineral fuels.

5. The application according to claim 1, characterized in that, The catalyst is suitable for use in the catalytic oxidation of CO within a temperature range of 0-800℃.

Citation Information

Patent Citations

  • Preparation method for AuAg@SiO2 nanometer catalyst of catalytic oxidation CO

    CN107519871A

  • Method for realizing in-situ growth of cobalt-manganese double-metal hydroxide composite material through using nickel foam as substrate

    CN108615610A

  • Oxide-modified Pt-Co bimetallic catalyst, preparation method and application of oxide-modified Pt-Co bimetallic catalyst in CO oxidation

    CN110876943A

  • Ozone room temperature decomposition honeycomb module and preparation method thereof

    CN110975610A

  • CO oxidation catalyst with high thermal stability as well as preparation method and application thereof

    CN111659382A