Back contact solar cell and method for preparing the same
By alternately arranging doping type areas and forming V-shaped trenches on the back side of the silicon-based substrate of the back-contact solar cell, filling multiple organic material layers, and combining laser technology to simplify the production process, the problems of high production cost and packaging short circuit risk are solved. Improved photoelectric conversion efficiency and battery reliability.
Patent Information
- Application Number
- CN202411003901.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-25
AI Technical Summary
The production process of back-contact solar cells is complex and costly, and there is a risk of short circuit during the packaging process, affecting cell performance and safety.
The first and second doped type regions are alternately arranged on the back side of the silicon-based substrate, and a V-shaped trench is formed therebetween, filled with multiple organic material layers, and doped and trenched through laser irradiation and etching. Simplify production processes and improve packaging reliability.
Effectively reduce light reflection and refraction loss, increase light absorption rate, enhance light propagation path, reduce production costs, simplify equipment configuration and process flow, and improve battery reliability and safety.
Smart Images

Figure CN118538779B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of solar cells, and in particular to a back-contact solar cell and a method for preparing the same. Background Art
[0002] As the global demand for clean energy continues to grow, solar energy, as a green and renewable energy source, has received widespread attention. As an important branch of solar cell technology, back contact solar cells (BC cells) have aroused heated discussions and in-depth research in the photovoltaic field with their unique design and significant performance advantages. In recent years, back contact solar cell technology has made significant progress. Its design concept is to place the positive and negative electrodes of the solar cell on the back of the cell, thereby realizing a grid-free design on the front of the cell, greatly reducing the shielding of the incident light by the grid lines in traditional cells and improving the photoelectric conversion efficiency. At the same time, the back contact structure also makes the battery packaging easier, improving the packaging density and aesthetics.
[0003] Although back-contact solar cell technology has achieved remarkable achievements, it still faces some urgent problems. First, the production process of back-contact solar cells is relatively complex, and the requirements for equipment and precision are high, which leads to high production costs and difficulty in large-scale promotion and application. Therefore, how to reduce production costs and improve production efficiency is one of the important challenges currently facing back-contact solar cell technology. Secondly, there is a risk of short circuit in the packaging process of back-contact solar cells. Since the positive and negative electrodes of the back-contact cell are both located on the back, if the packaging is improper or the material selection is inappropriate, it is easy to cause a short circuit between the electrodes, affecting the performance and safety of the battery. Therefore, how to improve the packaging process and materials and improve the reliability and safety of the battery is an issue that needs further research in back-contact solar cell technology. Summary of the invention
[0004] The purpose of the present application is to provide a back-contact solar cell, which can give full play to the structural advantages of the back-contact solar cell, and at the same time, the solar cell under the structure can be manufactured using a simple manufacturing method to reduce production costs. The structure of the back-contact solar cell of the present application includes a silicon-based substrate, and the back of the silicon-based substrate includes a first doping type region and a second doping type region, and the first doping type region and the second doping type region are alternately arranged;
[0005] The first doping type region is higher than the second doping type region, and a V-shaped groove is included between the first doping type region and the second doping type region;
[0006] The V-shaped groove is filled with multiple layers of organic material, and the refractive index of the multiple layers of organic material decreases from the silicon-based substrate outwards;
[0007] The size of the texturing on at least one side of the V-shaped groove gradually decreases from the bottom to the outside.
[0008] In one embodiment, the silicon-based substrate is N-type doped, the first doping type is P-type, and the second doping type is N-type.
[0009] In one embodiment, the doping concentration in the first doping type region and the second doping type region gradually decreases from the center of the region to both sides and inward.
[0010] In one of the embodiments, the outermost layer of the multi-layer organic material layer is flush with the second doping type region.
[0011] In one embodiment, the outermost organic material of the multi-layer organic material layer is an EVA derivative.
[0012] In one of the embodiments, one side of the V-shaped groove is perpendicular to the silicon-based substrate.
[0013] In one of the embodiments, the side perpendicular to the silicon-based substrate is located on one side of the second doping type region.
[0014] The present application further provides a method for preparing a back-contact solar cell, comprising:
[0015] Coating slurries of different doping types on the back side of the silicon-based substrate, wherein the slurries of different doping types correspond to the first doping type region and the second doping type region;
[0016] Use laser to irradiate different doping type slurry areas, the laser is a linear laser and the irradiation positions are respectively in the middle area of the first doping type area and the second doping type area;
[0017] Using laser etching to form a groove between the first doping type region and the second doping type region;
[0018] After etching to form the grooves, an organic coating is performed;
[0019] Wherein, the same laser optical path is used for laser doping and trench etching, and the optical path is offset by half the width of the first doping type region or the second doping type region.
[0020] In one of the embodiments, the method further includes forming a passivation layer and an anti-reflection layer.
[0021] In one embodiment, the silicon-based substrate is N-type doped, and before coating the slurry of different doping types, the silicon-based substrate is further doped with boron, and the doping concentration is greater than the doping concentration of the silicon-based substrate.
[0022] Compared with the prior art, the present application has the following beneficial effects: The present application provides a back-contact solar cell, including a silicon-based substrate, on the back of which a first doping type region and a second doping type region are alternately arranged, and a V-shaped groove is formed between the first doping type region and the second doping type region. The design of the V-shaped groove and the filling of multiple layers of organic material layers can effectively reduce the reflection and refraction loss of light and improve the absorption rate of light. The size of the V-shaped groove side velvet gradually decreases from the bottom to the outside, which can enhance the propagation path of light inside the solar cell, enhance the light trapping effect, and directly use the structure for optical alignment of the device without setting additional alignment marks. In addition, the present application adopts a laser-based manufacturing method. Due to the setting of the above-mentioned structure, different effects can be achieved by adjusting the energy of the laser, which can greatly reduce the structure and investment of the device. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 is a schematic structural diagram of a back-contact solar cell in one embodiment of the present application;
[0024] Figure 2 It is a schematic structural diagram of a back-contact solar cell in another embodiment of the present application.
[0025] Description of the reference numerals: 100, silicon-based substrate; 200, first doping type region; 300, second doping type region; 400, V-shaped groove. DETAILED DESCRIPTION
[0026] In order to make the above-mentioned purposes, features and advantages of the present application more obvious and easy to understand, the specific implementation methods of the present application are described in detail below in conjunction with the accompanying drawings. It is to be understood that the specific embodiments described herein are only used to explain the present application, rather than to limit the present application. It should also be noted that, for ease of description, only some structures related to the present application are shown in the accompanying drawings, rather than all structures. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0027] The terms "including" and "having" and any variations thereof in this application are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device comprising a series of steps or units is not limited to the listed steps or units, but may optionally include steps or units not listed, or may optionally include other steps or units inherent to these processes, methods, products or devices.
[0028] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0029] See also Figure 1 A back-contact solar cell in a preferred embodiment of the present application can simplify the manufacturing method of the back-contact solar cell structure, and reduce the production cost as much as possible on the basis of giving full play to the advantages of the back-contact solar cell structure. The back-contact solar cell of the present application includes a silicon-based substrate 100, and the back side of the silicon-based substrate 100 includes a first doping type region 200 and a second doping type region 300, and the first doping type region 200 and the second doping type region 300 are arranged alternately and at intervals. The back-contact solar cell is based on the silicon-based substrate 100, and the back side of the silicon-based substrate 100 is divided into a plurality of first doping type regions 200 and second doping type regions 300 that are arranged alternately and at intervals. This structure, as the main functional structure of the back-contact solar cell, realizes that all electrodes are set on the back side of the solar cell, and there is no need to form electrodes on the front side, thereby avoiding the front side from blocking light.
[0030] The first doping type region 200 is higher than the second doping type region 300. A V-shaped groove 400 is included between the first doping type region 200 and the second doping type region 300. Through the design of the V-shaped groove 400, the back contact solar cell can more effectively capture and utilize light energy, thereby improving the photoelectric conversion efficiency.
[0031] The V-shaped groove 400 is filled with multiple layers of organic material, and the refractive index of the multiple layers of organic material decreases from the silicon-based substrate 100 to the outside. Inside the V-shaped groove 400, multiple layers of organic material are filled, and the refractive index of these organic material layers decreases from the silicon-based substrate 100 to the outside. This gradient refractive index design effectively reduces the reflection and refraction loss of light, thereby improving the light absorption rate. In addition, filling the V-shaped groove 400 during the process of making the battery cell can avoid additional displacement of the encapsulation film during the subsequent component production process, and can also prevent bubbles from being left in the V-shaped groove 400.
[0032] The texturing size of at least one side of the V-shaped groove 400 gradually decreases from the bottom to the outside. The texturing method can adopt a dry ion etching method, and different texturing sizes can be produced by adjusting the process parameters. Due to the change of the texturing size, different optical stripes can be automatically generated during alignment in automated equipment. In a further embodiment, the width of part of the first doping type area 200 and the second doping type area 300 can be increased, while the width of the V-shaped groove 400 between the two can be reduced. In this way, characteristic stripes are generated, which is more conducive to optical alignment. The design of the texturing of the side of the V-shaped groove 400 makes the optical alignment process of the equipment simpler, without the need for additional alignment marks, thereby improving production efficiency.
[0033] Specifically, the silicon-based substrate is N-type doped, the first doping type is P-type, and the second doping type is N-type. The N-type doping of the silicon-based substrate is to add a small amount of pentavalent phosphorus into the silicon crystal, and the element replaces some silicon atoms in the silicon crystal, thereby forming free electrons (i.e., negative charges) in the silicon crystal, making the silicon-based substrate have negative conductivity. The N-type silicon substrate has a higher electron mobility and can collect and transmit electrons more effectively. By alternately arranging P-type and N-type doping regions on the N-type doped silicon-based substrate, multiple PN junctions can be formed, which can effectively convert light energy into electrical energy.
[0034] In a further embodiment, the doping concentration in the first doping type region 200 and the second doping type region 300 gradually decreases from the center of the region to both sides and inward. The structure has a high doping concentration in some areas, achieving the technical effect of discovering the emitter. The selective emitter improves the efficiency of the solar cell by forming different doping concentrations in the emitter region. The area with high doping concentration has better current collection ability, while the area with low doping concentration can reduce surface recombination loss. In the present application, the gradient doping method is used to ensure the effective collection of current and reduce surface recombination loss. In the preparation method, it can be achieved by laser doping technology in a simple method. Laser doping is a method of forming a specific doping type area in the silicon-based substrate by irradiating the surface of the silicon-based substrate with a laser beam to diffuse the doping elements into the silicon-based substrate. Since the laser energy only irradiates the central area, different temperature states will be generated on one surface, and the doping concentration will be different. By precisely controlling the energy of the laser beam, the effect of gradient changes with different doping concentrations can be achieved.
[0035] Specifically, the outermost layer of the multi-layer organic material layer is flush with the second doping type region 300. Since the multi-layer organic material layer reduces the reflection and refraction loss of light through the refractive index gradient, the organic material is prevented from contacting the surfaces of the first doping type region 200 and the second doping type region 300 in the above manner, thereby avoiding possible defects in subsequent electrode connections. A specific manufacturing method may be that after the organic material layer is formed as a whole, a solution dissolution method is used. Since the material in the V-groove 400 is difficult to directly contact the solution, the organic material in the V-groove 400 is maintained by controlling the time.
[0036] In order to make the connection of photovoltaic modules more stable, the organic material of the outermost layer of the multi-layer organic material layer is an EVA derivative. The choice of this special material enables this layer to be better combined with the EVA film used during packaging, so that the solar cells have higher overall strength after packaging, which helps to resist the impact and vibration of the external environment. At the same time, the good combination between the EVA derivative and the encapsulation EVA film can also reduce defects and stress concentration at the interface.
[0037] See also Figure 2 , Figure 2 It is a schematic diagram of the structure of a back-contact solar cell in another embodiment of the present application. In this embodiment, one side of the V-shaped groove 400 is perpendicular to the silicon-based substrate 100. Specifically, the side perpendicular to the silicon-based substrate 100 is located on one side of the second doping type region 300. By setting one side of the V-shaped groove 400 to be perpendicular to the silicon-based substrate 100, and the vertical side is located on one side of the second doping type region 300 (N-type region), the second doping type region 300 (N-type region) mainly plays the role of collecting current in the solar cell. By avoiding the incidence of light in this area, the current disturbance caused by illumination can be reduced, and the light is incident as much as possible into the area with the PN junction, which can effectively control the incident position and path of the light inside the solar cell, reduce light loss, optimize current collection, and enhance light absorption.
[0038] The present application further provides a method for preparing a back-contact solar cell, comprising:
[0039] Different doping types of slurries are coated on the back of the silicon-based substrate 100. The slurry coating technology is very mature in the field of solar cells, and the relevant equipment and processes have been widely studied. Different doping types of slurries correspond to the first doping type area 200 and the second doping type area 300. The different doping types of the present application are formed by combining doping slurries with laser diffusion, which can avoid the use of different masks or repeated etching steps; unlike traditional masks or repeated etching steps, the present application uses doping slurries combined with laser diffusion to achieve doping in different areas, which can greatly simplify the implementation of different doping types, which is both efficient and accurate, and can ensure the accuracy and uniformity of the doping area. In addition, during the laser doping process, heating can also be used to assist doping of dopants.
[0040] Laser is used to irradiate the slurry areas of different doping types. The laser is a linear laser and the irradiation position is respectively in the middle area of the first doping type area 200 and the second doping type area 300. Laser etching is used to etch a groove between the first doping type area 200 and the second doping type area 300. The laser method can achieve precise doping and groove etching.
[0041] After the grooves are formed by etching, organic coating is performed. The relevant functions of the organic matter have been explained above and will not be further discussed in detail here.
[0042] The same laser optical path is used for laser doping and groove etching, and the optical path is offset by half the width of the first doping type region 200 or the second doping type region 300. In this process, only the energy, action time and other parameters of the laser need to be adjusted. By offsetting the optical path by half the width of the first doping type region 200 or the second doping type region 300, different effects of the laser can be achieved by adjusting the laser energy, and no additional design template is required. The design of the same laser optical path makes the equipment configuration simpler and improves the flexibility and scalability of production.
[0043] In the solution based on this application, there is no need for a high-temperature diffusion furnace, and laser equipment, coating equipment, etc. can be used universally. The relevant equipment is mature, and only the materials and parameters of the relevant equipment need to be adaptively adjusted. There is no need for large-scale transformation of the equipment architecture or structure, which can simplify manufacturing costs.
[0044] Specifically, it also includes the steps of forming a passivation layer and an anti-reflection layer. The passivation layer is an oxide layer or a nitride layer formed on the surface of the solar cell, which reduces the surface active sites to achieve passivation, and the anti-reflection layer can reduce the reflection loss of light, so that more light can enter the interior of the solar cell. The materials, formation methods and formation positions of the passivation layer and the anti-reflection layer can be set according to the existing relevant contents in the field of solar cells. For this application, the relevant structures are especially made on the front side.
[0045] Specifically, the silicon-based substrate 100 is N-type doped, and before coating the slurry of different doping types, the silicon-based substrate 100 is also doped with boron, and the doping concentration is greater than the doping concentration of the silicon-based substrate 100. By doping the silicon-based substrate 100 in advance and forming an N-type heavily doped area in advance, the N-type doping can be made more controllable, and only P-type doping slurry can be coated in the slurry coating step.
[0046] As can be seen from the foregoing, the present invention proposes a back-contact solar cell structure and a method for preparing the same. This design ensures the photoelectric conversion efficiency of the solar cell while reducing the production cost by optimizing the structure and adopting a matching process. The back-contact solar cell of the present application is based on a silicon-based substrate. By alternately arranging the first doping type region and the second doping type region on the back of the substrate, the back area of the silicon-based substrate is fully utilized, and no grid lines that block light are formed on the front. The V-shaped grooves formed and the multi-layer organic material layers filled therein significantly reduce the reflection and refraction losses of light, thereby improving the absorption rate of light and optimizing the capture and utilization of light. The refractive index gradient design of the multi-layer organic material layers also achieves more efficient light propagation, while also avoiding the generation of bubbles in the groove position during the component manufacturing process.
[0047] In addition, the design of the V-groove side texture gradually decreasing in size from the bottom to the outside not only enhances the way light propagates inside the solar cell and improves the light trapping effect, but also allows the structure itself to be used for optical alignment of the device without the need for additional alignment marks, further simplifying the manufacturing process. In terms of preparation methods, the present invention adopts a laser-based manufacturing technology, which achieves doping of different areas of the silicon-based substrate and etching of the V-grooves by adjusting the energy of the laser, thereby ensuring the accuracy and stability of the structure. At the same time, this manufacturing method also simplifies the process flow, reduces equipment investment and production costs. In summary, the back-contact solar cell of the present application has been improved in terms of structural design, optical performance, and preparation process, ensuring high photoelectric conversion efficiency and low production costs.
[0048] The above is only a specific implementation of the present application, and any other improvements made based on the concept of the present application are deemed to be within the protection scope of the present application.
Claims
1. A back contact solar cell, characterized in that: The method comprises a silicon-based substrate, wherein the back side of the silicon-based substrate comprises a first doping type region and a second doping type region, wherein the first doping type region and the second doping type region are alternately arranged, and the first doping type region and the second doping type region are formed by laser irradiation of different doping type coating slurries; The first doping type region is higher than the second doping type region, and a V-shaped groove is included between the first doping type region and the second doping type region, wherein the V-shaped groove is formed by laser etching; The V-shaped groove is filled with multiple layers of organic material, and the refractive index of the multiple layers of organic material decreases from the silicon-based substrate outwards; The size of the texturing on at least one side of the V-shaped groove gradually decreases from the bottom to the outside.
2. The back contact solar cell according to claim 1, characterized in that: The silicon-based substrate is N-type doped, the first doping type is P-type, and the second doping type is N-type.
3. The back contact solar cell according to claim 2, characterized in that: The doping concentration in the first doping type region and the second doping type region gradually decreases from the center of the region to both sides and inward.
4. The back contact solar cell according to claim 1, characterized in that: The outermost layer of the multi-layer organic material layer is flush with the second doping type region.
5. The back contact solar cell according to claim 4, characterized in that: The outermost organic material of the multi-layer organic material layer is an EVA derivative.
6. The back contact solar cell according to claim 3, characterized in that: One side of the V-shaped groove is perpendicular to the silicon-based substrate.
7. The back contact solar cell according to claim 1, characterized in that: The side edge perpendicular to the silicon-based substrate is located on one side of the second doping type region.
8. A method for preparing a back contact solar cell, characterized in that: include: Coating slurries of different doping types on the back side of the silicon-based substrate, wherein the slurries of different doping types correspond to the first doping type region and the second doping type region; Use laser to irradiate different doping type slurry areas, the laser is a linear laser and the irradiation positions are respectively in the middle area of the first doping type area and the second doping type area; Using laser etching, a groove is formed between the first doping type region and the second doping type region, wherein the formed groove is a V-shaped groove; The texturing is performed by ion etching, and the texturing size of at least one side of the V-shaped groove is gradually reduced from the bottom to the outside; After etching to form the groove, organic coating is performed, wherein multiple layers of organic material are filled in the V-shaped groove, and the refractive index of the multiple layers of organic material decreases from the silicon-based substrate outwards; Wherein, the same laser optical path is used for laser doping and trench etching, and the optical path is offset by half the width of the first doping type region or the second doping type region.
9. The method for preparing a back contact solar cell according to claim 8, characterized in that: The method also includes the steps of forming a passivation layer and an anti-reflection layer.
10. The method for preparing a back contact solar cell according to claim 8, characterized in that: The silicon-based substrate is N-type doped, and before coating the slurry of different doping types, the silicon-based substrate is also doped with boron, and the doping concentration is greater than the doping concentration of the silicon-based substrate.
Citation Information
Patent Citations
A solar cell module with high conversion efficiency
CN102280512A
Packaged solar cell wafer and manufacturing method thereof
CN103107206A
Compound middle reflecting layer for battery and multi-junction multi-lamination silicon-based thin-film battery
CN103579400A
Silicon solar energy cell based on organic passivation film