Modified lithium-rich manganese-based material, preparation method, positive electrode material, positive electrode sheet and battery

By introducing Na+ and doping elements into lithium-rich manganese-based materials, and using poly-alkali metal phosphates to coat double-alkali metal lithium-rich oxides, a modified lithium-rich manganese-based material is formed, which solves the energy problem of traditional lithium-rich manganese-based materials. The problems of low density, poor cycle performance and high cost have been achieved to achieve efficient and stable lithium-ion battery performance.

CN118553892BActive Publication Date: 2024-10-29NINGBO RONBAY LITHIUM BATTERY MATERIAL CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410880061.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-29
Estimated Expiration
2044-07-02

AI Technical Summary

Technical Problem

Traditional lithium-rich manganese-based materials have problems such as low energy density, poor cycle performance, and high cost, which limit their commercial application.

Method used

Double alkali metal manganese-rich oxide is used as the core, and polyalkali metal phosphate is used as the ion conductor layer. The structural stability and electrochemical performance of the material are improved by introducing Na+ and doping elements to form a modified lithium-rich manganese-based material.

Benefits of technology

It improves the first Coulombic efficiency, discharge capacity, rate performance and cycle stability of the material, while reducing the cost, making it suitable as a high-performance cathode material for lithium-ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118553892B_ABST
    Figure CN118553892B_ABST
Patent Text Reader

Abstract

The present application relates to a modified lithium-rich manganese-based material, a preparation method, a positive electrode material, a positive electrode sheet and a battery. The modified lithium-rich manganese-based material comprises a core and an ion conductor layer covering the core, wherein the mass ratio of the core to the ion conductor layer is 100:(0.05-2); the core comprises a double alkali metal manganese-rich oxide, and the expression of the double alkali metal manganese-rich oxide is: Li a Na b Ni x Co y Mn z R 1‑x‑y‑z O c X d The ion conductor layer includes a polyalkali metal phosphate, and the expression of the polyalkali metal phosphate is: Li e Na f K h M2(PO4)3. The modified lithium-rich manganese-based material provided in the present application has the advantages of high discharge capacity, good rate performance, excellent cycle stability and low cost, and is very suitable as a positive electrode material for lithium-ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium-ion batteries, and in particular to a modified lithium-rich manganese-based material, a preparation method, a positive electrode material, a positive electrode sheet and a battery. Background Art

[0002] Lithium-ion batteries are widely used in 3C products, energy storage systems and power batteries due to their high energy density, long cycle life and good rate performance. How to further improve the energy density and cycle life of lithium-ion batteries has also become a research hotspot in the field of lithium-ion batteries. As the core part of lithium-ion batteries, positive electrode materials play a vital role in the preparation of high-performance lithium-ion batteries.

[0003] Currently, the commonly used positive electrode materials are lithium cobalt oxide (LiCoO2, LCO), nickel cobalt manganese ternary material (LiNi x Co y Mn 1-x- y O2, NCM), nickel-cobalt-aluminum ternary materials (LiNi x Co y Al 1-x-y O2, NCA), lithium iron phosphate (LiFePO4, LFP) and lithium manganese oxide (LiMn2O4, LMO). Among them, lithium-rich manganese-based materials (Li-rich NCM) have high manganese content and low nickel and cobalt content, and there are two charge compensation mechanisms of anions and cations. Compared with cobalt-based materials and nickel-based materials, they have higher specific capacity and lower cost. However, traditional lithium-rich manganese-based materials still have problems such as low energy density, poor cycle performance and high cost, which limit the commercial application of lithium-rich manganese-based materials. Summary of the invention

[0004] Based on this, it is necessary to provide a modified lithium-rich manganese-based material, a preparation method, a positive electrode material, a positive electrode sheet and a battery to overcome the problems of low energy density, poor cycle performance and high cost of traditional lithium-rich manganese-based materials.

[0005] In a first aspect of the present application, a modified lithium-rich manganese-based material is provided, comprising a core and an ion conductor layer covering the core, wherein the mass ratio of the core to the ion conductor layer is 100:(0.05-2);

[0006] The inner core includes a double alkali metal manganese-rich oxide, and the expression of the double alkali metal manganese-rich oxide is:

[0007] Li a Na b Ni x Co y Mn z R1-x-y-z O c X d ;

[0008] Among them, 1.1 <a<1.5,0.03<b≤0.3,0≤d≤0.1,a+b+1=c+d;

[0009] 0.25≤x≤0.4, 0≤y≤0.1, 0.6≤z≤0.75, 0<1-xyz≤0.05;

[0010] The R element includes one or more of Ca, Al, Ba, Ce, Cr, Cu, Fe, K, La, Mg, Mo, Te, Nb, Sb, Sm, Ta, Ti, V, W, Y, Sn, Zn and Zr;

[0011] The X element includes one or more of F, Cl and S;

[0012] The ion conductor layer includes a polyalkali metal phosphate, and the polyalkali metal phosphate is expressed as:

[0013] Li e Na f K h M2(PO4)3;

[0014] Among them, 0.5≤e≤2.3, 0.5≤f≤2.3, 0 <h≤0.2,e+f+h=3;

[0015] The M element includes one or more of Al, V, Cr, La and Y.

[0016] In one embodiment, the R element includes one or more of Nb, W, Mo, Sb, Cr and Zr.

[0017] In one embodiment, the M element includes one or more of V and Al.

[0018] In one embodiment, the thickness of the ion conductor layer is 5 nm to 20 nm.

[0019] In one embodiment, the median particle size of the ion conductor layer is less than 1 μm.

[0020] In one of the embodiments, the median particle size of the modified lithium-rich manganese-based material is 2 μm to 15 μm.

[0021] In a second aspect of the present application, a method for preparing a modified lithium-rich manganese-based material is provided, comprising the following steps:

[0022] Mixing a double alkali metal manganese-rich oxide and a polyalkali metal phosphate, and performing a second sintering treatment so that the polyalkali metal phosphate covers the double alkali metal manganese-rich oxide;

[0023] The mass ratio of the double alkali metal manganese-rich oxide to the polyalkali metal phosphate is 100:(0.05-2);

[0024] The double alkali metal manganese-rich oxide is expressed as: Li a Na b Ni x Co y Mn z R 1-x-y-z O c X d ;

[0025] Among them, 1.1 <a<1.5,0.03<b≤0.3,0≤d≤0.1,a+b+1=c+d;

[0026] 0.25≤x≤0.4, 0≤y≤0.1, 0.6≤z≤0.75, 0<1-xyz≤0.05;

[0027] The R element includes one or more of Ca, Al, Ba, Ce, Cr, Cu, Fe, K, La, Mg, Mo, Te, Nb, Sb, Sm, Ta, Ti, V, W, Y, Sn, Zn and Zr;

[0028] The X element includes one or more of F, Cl and S;

[0029] The polyalkali metal phosphate is expressed as: Li e Na f K h M2(PO4)3;

[0030] Among them, 0.5≤e≤2.3, 0.5≤f≤2.3, 0 <h≤0.2,e+f+h=3;

[0031] The M element includes one or more of Al, V, Cr, La and Y.

[0032] In one embodiment, the R element includes one or more of Nb, W, Mo, Sb, Cr and Zr.

[0033] In one embodiment, the M element includes one or more of V and Al.

[0034] In one embodiment, the second sintering process comprises the following steps:

[0035] Keep warm at 300℃~800℃ for 3h~15h.

[0036] In one embodiment, the preparation method of the double alkali metal manganese-rich oxide comprises the following steps:

[0037] Mixing a nickel-cobalt-manganese precursor, a lithium salt, a sodium salt and a dopant, and performing a first sintering treatment to prepare an intermediate;

[0038] washing and drying the intermediate to prepare the double alkali metal manganese-rich oxide;

[0039] Wherein, the dopant includes an R source, or the dopant includes an R source and an X source.

[0040] In one embodiment, the nickel-cobalt-manganese precursor includes one or more of oxides, hydroxides, carbonates, oxalates and ethanolates containing nickel, cobalt and manganese elements.

[0041] In one embodiment, the lithium salt includes one or more of lithium carbonate, lithium hydroxide, lithium nitrate, lithium sulfate, lithium chloride and lithium fluoride.

[0042] In one embodiment, the sodium salt includes one or more of sodium carbonate, sodium hydroxide, sodium sulfate, sodium oxalate, sodium acetate, sodium chloride and sodium fluoride.

[0043] In one embodiment, the R source includes one or more of oxides, fluorides, hydroxides and ethanolates containing the R element;

[0044] In one embodiment, the X source includes one or more of fluoride, chloride and sulfide.

[0045] In one embodiment, the first sintering process comprises the following steps:

[0046] Keep warm at 300℃~800℃ for 0h~10h, and keep warm at 800℃~1000℃ for 4h~20h.

[0047] In one embodiment, the washing process comprises the following steps:

[0048] Wash with water at a temperature of 0℃~25℃ for 1min~10min, and dehydrate.

[0049] In a third aspect of the present application, a positive electrode material is provided, which is made of the modified lithium-rich manganese-based material as described above, or made of the modified lithium-rich manganese-based material prepared by the preparation method of the modified lithium-rich manganese-based material as described above.

[0050] In a fourth aspect of the present application, a positive electrode sheet is provided, comprising a positive electrode current collector and a positive electrode active layer covering the positive electrode current collector, wherein the positive electrode active layer comprises the positive electrode material as described above.

[0051] In a fifth aspect of the present application, a lithium-ion battery is provided, comprising the positive electrode sheet as described above.

[0052] This application has at least the following beneficial effects:

[0053] This application uses double alkali metal manganese-rich oxide as the core, which introduces Na into the traditional lithium-rich manganese-based material. + Replacement part Li + , so that the core forms a unique sodium-deficient P2-type composite phase containing a large number of vacancies, which is beneficial to improve the initial coulombic efficiency and cycle performance of the material, while achieving the purpose of reducing costs. Limiting the stoichiometric ratio of each element is beneficial to reducing the introduction of Na + The negative impact brought by the material can be avoided, and problems such as excessive residual alkali, poor structural stability and kinetic decline can be avoided. Using R elements for doping is beneficial to improving the structural stability of the core and promoting the capacity. Using X elements for doping is beneficial to promoting the reversibility of anion redox and improving the first coulomb efficiency and first effect.

[0054] At the same time, the present application uses polyalkali metal phosphate as the ion conductor layer. On the one hand, it has good structural stability. After coating the core, it can reduce the interface side reaction, inhibit the release of lattice oxygen of the material, and improve the structural stability and long cycle performance of the material. On the other hand, it is a NASICON configuration with a three-dimensional ion diffusion channel, which can conduct Li + Can also conduct Na + , excellent dynamics, ensuring Li + and Na + The rapid transmission of ions increases the discharge capacity, improves the ion diffusion rate and enhances the rate performance. The ion conductor layer also introduces an appropriate amount of K + , whose ionic radius is larger than Li + and Na + Larger, can expand the lattice volume, for Li + and Na + provides more space for diffusion, thereby improving rate performance; at high voltage, K + It can also play a supporting role to ensure the structural stability of the ion conductor layer in the deep lithium / sodium removal state, thereby improving the cycle stability. Therefore, the modified lithium-rich manganese-based material provided by the present application has the advantages of high first coulombic efficiency, high discharge capacity, good rate performance, excellent cycle stability and low cost, and is very suitable as a positive electrode material for lithium-ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] In order to more clearly illustrate the technical solutions in the embodiments of the present application and to more completely understand the present application and its beneficial effects, the following is a brief introduction to the drawings required for the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without creative work.

[0056] Figure 1 This is a SEM image of the modified lithium-rich manganese-based material of Example 2;

[0057] Figure 2 XRD diagrams of the modified lithium-rich manganese-based materials of Examples 1-2 and Comparative Example 1;

[0058] Figure 3 The first charge and discharge curve of the battery corresponding to Example 1 at 0.2C;

[0059] Figure 4 The first charge and discharge curve of the battery corresponding to Example 2 at 0.2C;

[0060] Figure 5 The first charge and discharge curve of the battery corresponding to Comparative Example 1 at 0.2C;

[0061] Figure 6 Graph showing the test results of the cycle stability of the batteries corresponding to Examples 1-2 and Comparative Example 1 at 1C. DETAILED DESCRIPTION

[0062] In order to facilitate the understanding of the present application, the present application is further described in detail below in conjunction with specific embodiments. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.

[0063] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.

[0064] In the present application, the meaning of "and / or" includes any and all combinations of one or more related listed items. "At least one" means more than one, such as one, two and more than two. "Multiple" or "several" means at least two, such as two, three, etc., and "multi-layer" means at least two layers, such as two layers, three layers, etc., unless otherwise clearly and specifically defined. In the description of the present application, "several" means at least one, such as one, two, etc., unless otherwise clearly and specifically defined.

[0065] When a numerical range is disclosed in this application, the above range is considered to be continuous and includes the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed in this application should be understood to include any and all subranges included therein.

[0066] Unless otherwise specified, all steps of the present application may be performed sequentially or randomly. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may also include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0067] In this application, "above" or "below" includes the number itself. For example, "1 below" includes 1.

[0068] The temperature parameters in this application, unless otherwise specified, are allowed to be either constant temperature treatment or to vary within a certain temperature range. It should be understood that the constant temperature treatment allows the temperature to fluctuate within the accuracy range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.

[0069] In the present application, room temperature refers to indoor temperature, normal temperature or general temperature. Generally speaking, the range of room temperature can be any one of the following temperature intervals: 23°C ± 2°C, 25°C ± 5°C or 20°C ± 5°C.

[0070] In this application, the layered transition metal oxide is a layered structure formed by alternating transition metal layers and alkali metal layers, which can be divided into P2 type and O3 type according to the arrangement and stacking order of oxygen atoms. Compared with the O3 phase, the sodium-deficient P2 phase is conducive to improving the first coulomb efficiency of the material, and has a lower diffusion barrier and higher ionic conductivity, and has better electrochemical performance. At the same time, the P2 phase has a higher sodium content than the O3 phase. + There will be no oxide layer slippage during the embedding and de-embedding process, and the structure is more stable.

[0071] In the present application, sodium super ion conductor (NASICON) is a type of polyanion material with three-dimensional ion diffusion channels that can achieve rapid ion conduction.

[0072] Lithium-rich manganese-based materials can be regarded as continuous solid solutions composed of Li2MnO3 and LiMO2 in different proportions, where M is Ni, Co or Mn. Lithium-rich manganese-based materials have high manganese content and low nickel and cobalt content, and are less expensive than cobalt-based materials and high nickel-based materials. Lithium-rich manganese-based materials have two charge compensation mechanisms, anion and cation, with a theoretical specific capacity of more than 250mAh / g, and have the advantages of high operating voltage, high safety and low pollution. They are regarded as the ideal choice for the next generation of lithium-ion battery positive electrode materials. However, lithium-rich manganese-based materials also have problems such as high cost due to the larger amount of lithium used, low first coulomb efficiency, and poor cycle performance.

[0073] In terms of cost, the lithium content in lithium-rich manganese-based materials is 20% to 50% higher than that of traditional nickel-cobalt-manganese ternary positive electrode materials. The cost advantage brought by low-priced manganese-rich materials will gradually weaken as the price of lithium salts increases. In terms of material performance, lithium-rich manganese-based materials will be accompanied by the release of lattice oxygen during the charging and discharging process, and their layered structure will transform into a spinel structure and then to a rock salt structure, resulting in a decrease in structural stability. The evolution of these crystal structures causes lithium-rich manganese-based materials to exhibit problems such as low coulombic efficiency, voltage decay, and poor cycle performance in electrochemical performance, which hinders their commercial application process.

[0074] Based on this, in the first aspect of the present application, a modified lithium-rich manganese-based material is provided to overcome the problems of low first coulombic efficiency, poor cycle performance and high cost existing in traditional lithium-rich manganese-based materials.

[0075] In some embodiments, the modified lithium-rich manganese-based material includes a core, and an ion conductor layer covering the core, and the mass ratio of the core to the ion conductor layer is 100:(0.05-2);

[0076] The inner core includes a double alkali metal manganese-rich oxide, and the expression of the double alkali metal manganese-rich oxide is:

[0077] Li a Na b Ni x Co y Mn z R 1-x-y-z O c X d ;

[0078] Among them, 1.1 <a<1.5,0.03<b≤0.3,0≤d≤0.1,a+b+1=c+d;

[0079] 0.25≤x≤0.4, 0≤y≤0.1, 0.6≤z≤0.75, 0<1-xyz≤0.05;

[0080] The R element includes one or more of Ca, Al, Ba, Ce, Cr, Cu, Fe, K, La, Mg, Mo, Te, Nb, Sb, Sm, Ta, Ti, V, W, Y, Sn, Zn and Zr;

[0081] The X element includes one or more of F, Cl, S and N;

[0082] The ion conductor layer includes a polyalkali metal phosphate, and the polyalkali metal phosphate is expressed as:

[0083] Li e Na f K h M2(PO4)3;

[0084] Among them, 0.5≤e≤2.3, 0.5≤f≤2.3, 0 <h≤0.2,e+f+h=3;

[0085] The M element includes one or more of Al, V, Cr, La and Y.

[0086] This application uses double alkali metal manganese-rich oxide as the core, which introduces Na into the traditional lithium-rich manganese-based material. + Replacement part Li + , which makes the core form a unique sodium-deficient P2-type composite phase containing a large number of vacancies, which is beneficial to improve the first coulombic efficiency and cycle performance of the material. + Can replace part of Li + , to achieve the purpose of reducing costs. Limiting the stoichiometric ratio of each element is beneficial to reduce the introduction of Na + The negative impact brought by the material can be avoided, and problems such as excessive residual alkali, poor structural stability and kinetic decline can be avoided. Using R elements for doping is beneficial to improving the structural stability of the core and promoting the capacity. Using X elements for doping is beneficial to promoting the reversibility of anion redox and improving the first coulomb efficiency and first effect.

[0087] At the same time, the present application uses polyalkali metal phosphate as the ion conductor layer. On the one hand, it has good structural stability. After coating the core, it can reduce the interface side reaction, inhibit the release of lattice oxygen of the material, and improve the structural stability and long cycle performance of the material. On the other hand, it is a NASICON configuration with a three-dimensional ion diffusion channel, which can conduct Li + Can also conduct Na + , excellent dynamics, ensuring Li + and Na + The rapid transmission of ions increases the discharge capacity, improves the ion diffusion rate and enhances the rate performance. The ion conductor layer also introduces an appropriate amount of K + , whose ionic radius is larger than Li + and Na+ Larger, can expand the lattice volume, for Li + and Na + provides more space for diffusion, thereby improving rate performance; at high voltage, K + It can also play a supporting role to ensure the structural stability of the ion conductor layer in the deep lithium / sodium removal state, thereby improving the cycle stability. Therefore, the modified lithium-rich manganese-based material provided by the present application has the advantages of high first coulombic efficiency, high discharge capacity, good rate performance, excellent cycle stability and low cost, and is very suitable as a positive electrode material for lithium-ion batteries.

[0088] It can be understood that the ion conductor layer can cover the core partially or completely. If the ion conductor layer partially covers the core, the ion conductor layer is loaded on part of the surface of the core to form a dispersed island structure. If the ion conductor layer completely covers the core, the ion conductor layer is loaded on all surfaces of the core to form a continuous film structure, which has a more significant effect on improving structural stability and long cycle performance.

[0089] As an example, the mass ratio of the core to the ion conductor layer can be 100:0.05, 100:0.08, 100:0.1, 100:0.2, 100:0.5, 100:0.8, 100:1, 100:1.2, 100:1.5, 100:1.8 or 100:2, and can further be 100:(0.5~1.5).

[0090] In the present application, the mass ratio of the core and the ion conductor layer is limited to 100:(0.05-2), so that the ion conductor layer can form a good coating effect on the surface of the core. If the mass ratio of the ion conductor layer is too low, it will affect the uniformity of the coating layer, resulting in an insignificant modification effect. If the mass ratio of the ion conductor layer is too high, the discharge capacity will decrease.

[0091] As an example, a may be 1.1, 1.15, 1.2, 1.25, 1.3, 1.35, 1.4 or 1.45. Further optionally, 1.2≤a≤1.3.

[0092] As an example, b may be 0.03, 0.05, 0.08, 0.1, 0.12, 0.14, 0.16, 0.18, 0.2, 0.22, 0.24, 0.26, 0.28 or 0.3. Further optionally, 0.05≤b≤0.15.

[0093] In the present application, by limiting the values ​​of a and b, the Li + and Na + molar ratio, avoiding Li + Dona +The purpose of reducing the cost cannot be achieved, and the Li + Shao Na + The defects of low discharge capacity and excessive residual alkali on the surface are caused by many factors.

[0094] As an example, d may be 0, 0.02, 0.04, 0.06, 0.08, or 0.1. Further optionally, 0.00≤d≤0.05.

[0095] In the present application, the values ​​of a, b, c and d satisfy the relationship of a+b+1=c+d. When the values ​​of a, b and d are determined, the value of c can also be determined.

[0096] As an example, x may be 0.25, 0.26, 0.27, 0.28, 0.29, 0.3, 0.32, 0.34, 0.36, 0.38 or 0.4. Further optionally, 0.28≤x≤0.35.

[0097] As an example, y may be 0, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09 or 0.1. Further optionally, 0.01≤y≤0.08.

[0098] As an example, z may be 0.6, 0.62, 0.64, 0.66, 0.68, 0.7, 0.71, 0.72, 0.73, 0.74 or 0.75. Further optionally, 0.63≤z≤0.7.

[0099] In the present application, by limiting the values ​​of x and z, the molar ratio of Ni and Mn in the double alkali metal manganese-rich oxide can be limited, which can avoid Ni being more than Mn, thereby not affecting Na + The embedding of Ni and Mn can reduce the residual alkali and improve the structural stability. On the other hand, it can reduce the defects of kinetic decline caused by less Ni and more Mn.

[0100] As an example, 1-xyz may be 0.005, 0.01, 0.015, 0.02, 0.025, 0.03, 0.035, 0.04, 0.045 or 0.05. Further optionally, 0.005≤1-xyz≤0.025.

[0101] In the present application, limiting 1-xyz to less than 0.05 can ensure that the transition metal ions have a suitable doping amount and avoid the defect of excessive doping amount causing the generation of impurities and resulting in a decrease in discharge capacity.

[0102] As an example, e may be 0.5, 0.6, 0.8, 1, 1.2, 1.4, 1.6, 1.8, 2, 2.1, 2.2 or 2.3. Further optionally, 1≤e≤2.

[0103] As an example, f may be 0.5, 0.6, 0.8, 1, 1.2, 1.4, 1.6, 1.8, 2, 2.1, 2.2 or 2.3. Further optionally, 1≤f≤2.

[0104] In this application, by limiting the values ​​of e and f, the Li in the polyalkali metal phosphate can be limited. + and Na + molar ratio, avoiding Li + Dona + The purpose of reducing the cost cannot be achieved, and the reduction of Li + Shao Na + The defects of low capacity and excessive residual alkali are mostly caused by this.

[0105] As an example, h may be 0.01, 0.02, 0.04, 0.06, 0.08, 0.1, 0.12, 0.14, 0.16, 0.18 or 0.2. Further optionally, 0.05≤h≤0.15.

[0106] In this application, by limiting the value of h, it can be ensured that the ion conductor layer contains a sufficient amount of K + , in order to achieve the purpose of improving capacity, rate performance and cycle stability. At the same time, it can also prevent K + Too high a content may lead to Li + and Na + The ion diffusion channels are reduced, avoiding the decrease in discharge capacity and rate performance.

[0107] It can be understood that the R element can be selected from any one of Ca, Al, Ba, Ce, Cr, Cu, Fe, K, La, Mg, Mo, Te, Nb, Sb, Sm, Ta, Ti, V, W, Y, Sn, Zn and Zr, or can be selected from two or more of the above elements. Further optionally, the R element includes one or more of Nb, W, Mo, Sb, Cr and Zr. On the one hand, the above elements can be doped in the surface interface to refine the grains, and on the other hand, they can be doped in the bulk phase to stabilize the stability of the bulk phase structure. Further optionally, R is Nb.

[0108] It can be understood that the X element can be selected from any one of F, Cl, S and N, or can be selected from two or more of the above non-metallic elements. Further optionally, the X element is F.

[0109] It is understandable that the M element can be selected from any one of Al, V, Ti, Zr, Cr, La and Y, or can be selected from two or more of the above metal elements. Further optionally, the M element includes one or more of V and Al.

[0110] Optionally, the thickness of the ion conductor layer is 5 nm to 20 nm. If the ion conductor layer completely covers the inner core and is supported on all surfaces of the inner core to form a continuous film structure, the thickness of the ion conductor layer may be 5 nm, 6 nm, 7 nm, 8 nm, 9 nm, 10 nm, 11 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 17 nm, 18 nm, 19 nm or 20 nm.

[0111] Optionally, the median particle size (D50) of the ion conductor layer is less than 1 μm. If the ion conductor layer partially covers the core, and the ion conductor layer is supported on a portion of the surface of the core to form a dispersed island structure, the D50 of each island structure can be 10 nm, 20 nm, 50 nm, 80 nm, 100 nm, 200 nm, 500 nm, 800 nm, 900 nm. Further optionally, the D50 of the ion conductor layer is less than 200 nm.

[0112] Optionally, the median particle size (D50) of the modified lithium-rich manganese-based material is 2 μm to 15 μm. As an example, the D50 of the modified lithium-rich manganese-based material may be 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm or 15 μm.

[0113] In a second aspect of the present application, a method for preparing a modified lithium-rich manganese-based material is provided, which is used to prepare the modified lithium-rich manganese-based material as described above.

[0114] In some embodiments, the method for preparing the modified lithium-rich manganese-based material comprises the following steps:

[0115] Mixing a double alkali metal manganese-rich oxide and a polyalkali metal phosphate, and performing a second sintering treatment so that the polyalkali metal phosphate covers the double alkali metal manganese-rich oxide;

[0116] The mass ratio of double alkali metal manganese-rich oxide to polyalkali metal phosphate is 100:(0.05~2);

[0117] The expression of double alkali metal manganese-rich oxide is: Li a Na b Ni x Co y Mn z R 1-x-y-z O c X d ;

[0118] Among them, 1.1 <a<1.5,0.03<b≤0.3,0≤d≤0.1,a+b+1=c+d;

[0119] 0.25≤x≤0.4, 0≤y≤0.1, 0.6≤z≤0.75, 0<1-xyz≤0.05;

[0120] The R element includes one or more of Ca, Al, Ba, Ce, Cr, Cu, Fe, K, La, Mg, Mo, Te, Nb, Sb, Sm, Ta, Ti, V, W, Y, Sn, Zn and Zr;

[0121] The X element includes one or more of F, Cl and S;

[0122] The expression of polyalkali metal phosphate is: Li e Na f K h M2(PO4)3;

[0123] Among them, 0.5≤e≤2.3, 0.5≤f≤2.3, 0 <h≤0.2,e+f+h=3;

[0124] The M element includes one or more of Al, V, Cr, La and Y.

[0125] It can be understood that the mass ratio of the double alkali metal manganese-rich oxide and the polyalkali metal phosphate, the optional types of R element, X element and M element, and the values ​​of a, b, c, d, e, f, h, x, y and z are all as described above and will not be repeated here.

[0126] Optionally, the second sintering treatment includes the following steps: keeping warm at 300° C. to 800° C. for 3 h to 15 h.

[0127] As an example, the sintering temperature of the second sintering treatment may be 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C or 800°C, further optionally 350°C to 750°C, further optionally 450°C to 550°C.

[0128] In the present application, the sintering temperature of the second sintering treatment should not be too high, because the alkali metal vacancies in the material will be transformed into an inert rock salt phase at an excessively high sintering temperature, thereby causing a decrease in discharge capacity.

[0129] As an example, the holding time of the second sintering treatment can be 3h, 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h or 15h, and can further be 8h~12h.

[0130] Optionally, in the second sintering treatment, the heating rate from room temperature to the sintering temperature is 1°C / min to 10°C / min, for example, 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min or 10°C / min, and can be further optionally 2°C / min to 6°C / min.

[0131] Optionally, the second sintering process is performed in an oxygen-containing atmosphere, such as an air atmosphere.

[0132] Optionally, the preparation method of the double alkali metal manganese-rich oxide includes the following steps: mixing a nickel-cobalt-manganese precursor, a lithium salt, a sodium salt and a dopant, performing a first sintering treatment to prepare an intermediate; washing and drying the intermediate to prepare the double alkali metal manganese-rich oxide; wherein the dopant includes an R source, or the dopant includes an R source and an X source.

[0133] Optionally, the nickel-cobalt-manganese precursor includes one or more of oxides, hydroxides, carbonates, oxalates and ethanolates containing nickel, cobalt and manganese elements, and may further be a hydroxide containing nickel, cobalt and manganese elements.

[0134] Optionally, the molar ratio of nickel, cobalt and manganese in the nickel-cobalt-manganese precursor is (0.25-0.4):(0-0.1):(0.6-0.75), which is the same as the molar ratio of nickel, cobalt and manganese in the double alkali metal manganese-rich oxide.

[0135] Optionally, the ratio of the molar amount of lithium element in the lithium salt to the sum of the molar amounts of nickel element, cobalt element and manganese element in the nickel-cobalt-manganese precursor is: a / (x+y+z)=1.1~1.5; the ratio of the molar amount of sodium element in the sodium salt to the sum of the molar amounts of nickel element, cobalt element and manganese element in the nickel-cobalt-manganese precursor is b / (x+y+z)=0.03~0.3; the ratio of the molar amount of R element in the R source to the sum of the molar amounts of nickel element, cobalt element and manganese element in the nickel-cobalt-manganese precursor is (1-xyz) / (x+y+z)=0~0.05; the ratio of the molar amount of X element in the X source to the sum of the molar amounts of nickel element, cobalt element and manganese element in the nickel-cobalt-manganese precursor is d / (x+y+z)=0~0.1.

[0136] In the present application, during the washing process, the alkali metal sodium ions in the intermediate react with the H + Ion exchange is performed to reduce the alkali metal content in the water-washed product, so the sodium salt should be appropriately excessive so that the alkali metal content of the water-washed product is consistent with the alkali metal content of the target expression.

[0137] Optionally, the lithium salt includes one or more of lithium carbonate (Li2CO3), lithium hydroxide (LiOH), lithium nitrate (LiNO3), lithium sulfate (Li2SO4), lithium chloride (LiCl) and lithium fluoride (LiF), and further lithium carbonate (Li2CO3) may be selected. The raw material of the lithium salt may contain bound water, such as lithium hydroxide monohydrate (LiOH•H2O), or may not contain bound water, such as anhydrous lithium carbonate.

[0138] Optionally, the sodium salt includes one or more of sodium carbonate (Na2CO3), sodium hydroxide (NaOH), sodium sulfate (Na2SO4), sodium oxalate (Na2C2O4), sodium acetate (CH3COONa), sodium chloride (NaCl) and sodium fluoride (NaF), and further sodium carbonate (Na2CO3) may be selected. The raw material of the sodium salt may also contain bound water, such as sodium carbonate monohydrate or sodium carbonate decahydrate, or may not contain bound water, such as anhydrous sodium carbonate.

[0139] Optionally, the R source includes one or more of an oxide, a fluoride, a hydroxide and an ethoxide containing an R element. Further optionally, the R source is an oxide containing an M element, such as one or more of CaO, Al2O3, BaO, CeO2, Cr2O3, CuO, Fe2O3, K2O, La2O3, MgO, MoO3, TeO2, Nb2O5, Sb2O5, Sm2O3, Ta2O5, TiO2, V2O5, WO3, Y2O5, SnO2, ZnO and ZrO2. Further optionally, the R source is one or more of Nb2O5, WO3, MoO3, Sb2O5, Cr2O3 and ZrO2.

[0140] Optionally, the X source includes one or more of fluoride, chloride and sulfide. Among them, the fluoride includes one or more of NaF, LiF, KF and NH4F; the chloride includes one or more of NaCl, LiCl, KCl and NH4Cl; the sulfide includes one or more of Li2S, Na2S and CH4N2S. Further optionally, the X source is a fluoride. Further optionally, the X source is NH4F.

[0141] Optionally, the first sintering treatment includes the following steps: keeping warm at 300°C-800°C for 0h-10h, and keeping warm at 800°C-1000°C for 4h-20h.

[0142] As an example, the first sintering temperature of the first sintering treatment may be 300°C, 350°C, 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C or 800°C, further optionally 350°C to 750°C, further optionally 450°C to 550°C.

[0143] In the present application, the sintering temperature of the first sintering treatment should not be too high, because at too high a sintering temperature, the sintered product will grow excessively, resulting in an increase in the particle size of the intermediate and an excessively high density, which will have a negative impact on the discharge capacity.

[0144] As an example, the holding time of the first sintering treatment at the first sintering temperature can be 0h, 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, 9h or 10h, and can further be 4h~8h.

[0145] As an example, the second sintering temperature of the first sintering treatment may be 800°C, 820°C, 850°C, 880°C, 900°C, 920°C, 950°C, 980°C or 1000°C, further optionally 900°C to 1000°C, and further optionally 940°C to 960°C.

[0146] As an example, the holding time of the first sintering treatment at the second sintering temperature can be 4h, 5h, 6h, 7h, 8h, 9h, 10h, 11h, 12h, 13h, 14h, 15h, 16h, 17h, 18h, 19h or 20h, and can further be 8h~15h.

[0147] Optionally, in the first sintering treatment, the heating rate from room temperature to the first sintering temperature and the heating rate from the first sintering temperature to the second sintering temperature are each independently 1°C / min to 10°C / min, for example, 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min or 10°C / min.

[0148] Optionally, the first sintering process is performed in an oxygen-containing atmosphere, such as an air atmosphere.

[0149] Optionally, the washing treatment includes the following steps: washing with water at a water temperature of 0°C to 25°C for 1 min to 10 min, and dehydrating.

[0150] As an example, the water in the washing process can be tap water, deionized water, pure water, ultrapure water, distilled water or reverse osmosis water, and can further be deionized water or pure water to reduce the introduction of impurities.

[0151] As an example, the water temperature for the washing process can be 0°C, 2°C, 5°C, 8°C, 10°C, 12°C, 15°C, 18°C, 20°C, 22°C, 24°C or 25°C, and can be further optionally 5°C~15°C.

[0152] As an example, the washing time of the washing treatment can be 1 min, 2 min, 3 min, 4 min, 5 min, 6 min, 7 min, 8 min, 9 min or 10 min, and can be further selected as 2 min to 8 min.

[0153] In this application, the water temperature for washing treatment should not be too high, because if the water temperature is too high, the alkali metal ions and H + The degree of exchange is too high, especially the excessive sodium-hydrogen exchange, which reduces the cycle stability; at the same time, the washing time has little effect on the electrochemical properties of the material, but too long washing time will reduce the actual production efficiency.

[0154] Optionally, the mass ratio of water to the intermediate in the washing treatment is (1-5):1, for example, 1:1, 1.5:1, 2:1, 2.5:1, 3:1, 3.5:1, 4:1, 4.5:1 or 5:1.

[0155] Optionally, the dehydration treatment method includes one or more of suction filtration, filter press and centrifugation.

[0156] Optionally, the drying process comprises the following steps: drying at 90° C. to 200° C. for 10 h to 24 h.

[0157] As an example, the drying method includes one or more of air-blast drying and vacuum drying.

[0158] As an example, the temperature of the drying process can be 90°C, 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C, 180°C, 190°C or 200°C, and can further be 90°C~150°C.

[0159] As an example, the drying time may be 10 h, 12 h, 14 h, 16 h, 18 h, 20 h, 22 h, 24 h, and may further be 12 h to 18 h.

[0160] In a third aspect of the present application, a positive electrode material is provided, which is made of the modified lithium-rich manganese-based material as described above, or made of the modified lithium-rich manganese-based material prepared by the preparation method of the modified lithium-rich manganese-based material as described above.

[0161] In a fourth aspect of the present application, a positive electrode sheet is provided, comprising a positive electrode current collector and a positive electrode active layer covering the positive electrode current collector, wherein the positive electrode active layer comprises the positive electrode material as described above.

[0162] It can be understood that the positive electrode active layer covers at least one surface of the positive electrode current collector, and may cover only one surface or two opposite surfaces at the same time to form a structure in which the positive electrode active layer, the positive electrode current collector and the positive electrode active layer are stacked in sequence.

[0163] Optionally, the positive electrode current collector includes a metal foil or a composite current collector. The metal foil may be aluminum foil; the composite current collector includes a polymer substrate and a metal layer formed on the polymer substrate, the polymer substrate may be made of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS) and polyethylene (PE), and the metal layer may be made of aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy.

[0164] Optionally, the positive electrode active layer includes a positive electrode material, a binder and a conductive agent. + and Na + The binder is used to improve the bonding strength between the positive electrode active layer and the positive electrode current collector, and the conductive agent is used to improve the conductive performance of the positive electrode active layer.

[0165] Optionally, in the positive electrode active layer, the mass ratio of the positive electrode material, the binder and the conductive agent is (80~95):(2~6):(2~6).

[0166] Optionally, the binder includes at least one of polyvinylidene fluoride (PVDF), sodium alginate (SA), polyvinyl alcohol (PVA), polymethyl methacrylate (PMMA), hydrogenated nitrile rubber (HNBR), polytetrafluoroethylene (PTFE), and polyacrylic acid (PAA).

[0167] Optionally, the conductive agent includes at least one of conductive carbon, superconducting carbon, acetylene black, carbon black, Ketjen black, carbon quantum dots, carbon nanotubes, graphene and carbon nanofibers.

[0168] Optionally, the preparation method of the positive electrode sheet includes the following steps: dispersing the positive electrode material, the conductive agent and the binder in an organic solvent to prepare a positive electrode slurry; covering the positive electrode slurry on at least one surface of the positive electrode current collector, and drying, rolling and cutting to obtain a positive electrode sheet. The organic solvent is selected from N-methylpyrrolidone (NMP); the solid content of the positive electrode slurry is 20% to 50%; the drying temperature is 100°C to 150°C, the time is 60min to 120min, and further optionally, drying at 120°C for 80min.

[0169] In a fifth aspect of the present application, a lithium-ion battery is provided, comprising the positive electrode sheet as described above.

[0170] As can be understood, lithium-ion batteries include positive and negative electrodes, electrolytes, and separators. During the charge and discharge cycle, active lithium ions are intercalated and deintercalated between the positive and negative electrodes; the electrolyte conducts lithium ions between the positive and negative electrodes; and the separator is located between the positive and negative electrodes to prevent short circuits while allowing lithium ions to pass through.

[0171] Optionally, the negative electrode sheet includes a negative electrode current collector and a negative electrode active layer covering at least one surface of the negative electrode current collector. The negative electrode current collector includes a metal foil or a composite current collector. The metal foil in the negative electrode current collector can be copper foil. The composite current collector in the negative electrode current collector is basically the same as the composite current collector selected for the positive electrode current collector, and will not be described in detail.

[0172] Optionally, the negative electrode active layer includes a negative electrode material, a binder and a conductive agent. The negative electrode material includes at least one of elemental silicon, silicon oxide, silicon-carbon composite, silicon-nitrogen composite, and silicon alloy material; the binder includes at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS); the conductive agent includes at least one of conductive carbon, superconducting carbon, acetylene black, carbon black, Ketjen black, carbon quantum dots, carbon nanotubes, graphene, and carbon nanofibers.

[0173] It is understood that the electrolyte in a lithium-ion battery can be liquid, gel or all-solid.

[0174] Optionally, the electrolyte adopts an electrolyte solution, which includes a lithium salt and an organic solvent. Among them, the lithium salt includes at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl imide), lithium bis(trifluoromethanesulfonyl imide), lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalate borate, lithium dioxalate borate, lithium difluorodioxalate phosphate and lithium tetrafluorooxalate phosphate; the organic solvent includes at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.

[0175] Optionally, the electrolyte further includes additives, such as negative electrode film-forming additives, positive electrode film-forming additives, additives for improving battery overcharge performance, additives for improving battery high or low temperature performance, etc.

[0176] It is understandable that the separator can be a porous separator with good chemical stability and mechanical stability; at the same time, the separator can be a single-layer film or a multi-layer composite film. When the separator is a multi-layer composite film, the materials of each layer can be the same or different, without special restrictions.

[0177] Optionally, the material of the diaphragm includes at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride.

[0178] It can be understood that the lithium-ion battery of the present application includes a battery cell form, a battery module form and a battery pack form. The shape of the lithium-ion battery can be cylindrical, square or other arbitrary shapes.

[0179] Optionally, the positive electrode sheet, the negative electrode sheet and the separator may be formed into an electrode assembly by a winding process or a lamination process.

[0180] Optionally, the lithium-ion battery may include an outer package for encapsulating the electrode assembly and the electrolyte. The outer package of the lithium-ion battery may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer package of the lithium-ion battery may also be a soft package, such as a bag-type soft package, and the material of the soft package may be plastic, such as polypropylene, polybutylene terephthalate, and polybutylene succinate, etc.

[0181] Optionally, the battery cells can be assembled into a battery module, and the number of battery cells contained in the battery module can be one or more. The battery modules can also be assembled into a battery pack, and the number of battery modules contained in the battery pack can be one or more.

[0182] Optionally, the battery cells, battery modules, and battery packs can be used as power sources for electrical devices or as energy storage units for electrical devices. Electrical devices include, but are not limited to: mobile devices, such as mobile phones, tablet computers, and laptop computers; electric vehicles, such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.; electric trains; ships; satellites; and energy storage systems.

[0183] The following is further described in conjunction with specific embodiments and comparative examples. The raw materials involved in the following specific embodiments and comparative examples, unless otherwise specified, can all be commercially available, the instruments used, unless otherwise specified, can all be commercially available, and the processes involved, unless otherwise specified, are all routinely selected by those skilled in the art.

[0184] Example 1

[0185] Please refer to Table 1, the preparation method of the modified lithium-rich manganese-based material of this embodiment is as follows:

[0186] (1) uniformly mixing a nickel-cobalt-manganese precursor, a lithium salt, a sodium salt and a dopant to obtain a mixture;

[0187] The nickel-cobalt-manganese precursor is nickel-cobalt-manganese hydroxide Ni 0.33 Co 0.01 Mn 0.66 (OH)2;

[0188] The lithium salt is lithium carbonate, and the molar ratio of each element satisfies: Li / (Ni+Co+Mn)=1.25;

[0189] The sodium salt is sodium carbonate, and the molar ratio of each element satisfies: Na / (Ni+Co+Mn)=0.25;

[0190] The dopant is Nb2O5, and the molar ratio of each element satisfies: Nb / (Ni+Co+Mn)=0.005.

[0191] (2) The mixed material is placed in an atmosphere box furnace for the first sintering treatment: the temperature is raised from room temperature to 500°C at a heating rate of 5°C / min and kept at this temperature for 5 h; the temperature is raised from 500°C to 950°C at a heating rate of 5°C / min and kept at this temperature for 15 h; the mixed material is naturally cooled to room temperature in the furnace to obtain an intermediate, the expression of which is:

[0192] Li 1.25 Na 0.25 Ni 0.33 Co 0.01 Mn 0.66 Nb 0.005 O 2.505 .

[0193] (3) The intermediate was mixed with deionized water and washed under stirring conditions: the water temperature was controlled at 10°C, the mass ratio of water to the intermediate was 2:1, and the washing time was 5 min; dehydration was performed by filtration, and vacuum drying was performed at 120°C for 12 h, and crushing was performed to obtain a double alkali metal manganese-rich oxide with D50 = 10 μm, whose expression is Li 1.244 Na 0.080 (Ni 0.33 Co 0.01 Mn 0.66 ) 0.995 Nb 0.005 O 2.324 (For the convenience of writing chemical formulas, keep three decimal places and round off to the nearest value).

[0194] (4) According to the mass ratio of 100:0.5, the double alkali metal manganese-rich oxide and the polyalkali metal phosphate Li 1.9 NeK 0.1V2(PO4)3 was mixed evenly, and the temperature was raised from room temperature to 500°C at a heating rate of 5°C / min, and kept warm for 10 hours for the second sintering treatment; it was naturally cooled to room temperature in the furnace, passed through a 300-mesh sieve, and a modified lithium-rich manganese-based material was obtained.

[0195] Example 2

[0196] The difference between this embodiment and embodiment 1 is that the dopants are Nb2O5 and NH4F, and the molar ratio of each element satisfies: Nb / (Ni+Co+Mn)=0.005, F / (Ni+Co+Mn)=0.02, and the mass ratio of the double alkali metal manganese-rich oxide and the polyalkali metal phosphate is 100:1.

[0197] Example 3

[0198] The difference between this embodiment and embodiment 1 is that the dopants are Nb2O5 and NH4F, and the molar ratio of each element satisfies: Nb / (Ni+Co+Mn)=0.005, F / (Ni+Co+Mn)=0.05, and the mass ratio of the double alkali metal manganese-rich oxide and the polyalkali metal phosphate is 100:2.

[0199] Example 4

[0200] The difference between this embodiment and embodiment 2 is that the doping agents are Nb2O5 and NH4F, and the molar ratio of each element satisfies: Nb / (Ni+Co+Mn)=0.005, F / (Ni+Co+Mn)=0.08, and the expression of the polyalkali metal phosphate is Li 1.9 NeK 0.1 V 1.8 Al 0.2 (PO4)3.

[0201] Example 5

[0202] The difference between this embodiment and embodiment 2 is that the sintering temperature in step (4) is 750°C.

[0203] Example 6

[0204] The difference between this embodiment and embodiment 2 is that the sintering temperature in step (4) is 350°C.

[0205] Example 7

[0206] The difference between this embodiment and embodiment 2 is that the expression of polyalkali metal phosphate is Li 2.3 Na 0.6 K 0.1 V2(PO4)3.

[0207] Example 8

[0208] The difference between this embodiment and embodiment 2 is that the expression of polyalkali metal phosphate is Li 0.6 Na 2.2 K 0.2 V2(PO4)3.

[0209] Example 9

[0210] The difference between this embodiment and embodiment 2 is that the raw materials in step (1) are different.

[0211] The nickel-cobalt-manganese precursor is nickel-cobalt-manganese hydroxide Ni 0.34 Mn 0.66 (OH)2;

[0212] The lithium salt is lithium carbonate, and the molar ratio of each element satisfies: Li / (Ni+Co+Mn)=1.24;

[0213] The sodium salt is sodium carbonate, and the molar ratio of each element satisfies: Na / (Ni+Co+Mn)=0.24;

[0214] The dopants are WO3 and NH4F, and the molar ratio of each element satisfies: W / (Ni+Co+Mn)=0.01, F / (Ni+Co+Mn)=0.02.

[0215] Example 10

[0216] The difference between this embodiment and embodiment 2 is that the raw materials in step (1) are different.

[0217] The nickel-cobalt-manganese precursor is nickel-cobalt-manganese hydroxide Ni 0.25 Mn 0.75 (OH)2;

[0218] The lithium salt is lithium carbonate, and the molar ratio of each element satisfies: Li / (Ni+Co+Mn)=1.4;

[0219] The sodium salt is sodium carbonate, and the molar ratio of each element satisfies: Na / (Ni+Co+Mn)=0.28;

[0220] The dopants are MoO3 and NH4F, and the molar ratio of each element satisfies: Mo / (Ni+Co+Mn)=0.02, F / (Ni+Co+Mn)=0.02.

[0221] Embodiment 11

[0222] The difference between this embodiment and embodiment 2 is that the raw materials in step (1) are different.

[0223] The nickel-cobalt-manganese precursor is nickel-cobalt-manganese hydroxide Ni 0.3 Mn 0.7 (OH)2;

[0224] The lithium salt is lithium carbonate, and the molar ratio of each element satisfies: Li / (Ni+Co+Mn)=1.3;

[0225] The sodium salt is sodium carbonate, and the molar ratio of each element satisfies: Na / (Ni+Co+Mn)=0.26;

[0226] The dopants are Sb2O5 and NH4F, and the molar ratio of each element satisfies: Sb / (Ni+Co+Mn)=0.02, F / (Ni+Co+Mn)=0.02.

[0227] Example 12

[0228] The difference between this embodiment and embodiment 2 is that the raw materials in step (1) are different.

[0229] The nickel-cobalt-manganese precursor is nickel-cobalt-manganese hydroxide Ni 0.37 Mn 0.63 (OH)2;

[0230] The lithium salt is lithium carbonate, and the molar ratio of each element satisfies: Li / (Ni+Co+Mn)=1.18;

[0231] The sodium salt is sodium carbonate, and the molar ratio of each element satisfies: Na / (Ni+Co+Mn)=0.22;

[0232] The dopants are Cr2O3 and NH4F, and the molar ratio of each element satisfies: Cr / (Ni+Co+Mn)=0.05, F / (Ni+Co+Mn)=0.02.

[0233] Embodiment 13

[0234] The difference between this embodiment and embodiment 2 is that the raw materials in step (1) are different.

[0235] The nickel-cobalt-manganese precursor is nickel-cobalt-manganese hydroxide Ni 0.4 Mn 0.6 (OH)2;

[0236] The lithium salt is lithium carbonate, and the molar ratio of each element satisfies: Li / (Ni+Co+Mn)=1.13;

[0237] The sodium salt is sodium carbonate, and the molar ratio of each element satisfies: Na / (Ni+Co+Mn)=0.2;

[0238] The dopants are ZrO2 and NH4F, and the molar ratio of each element satisfies: Zr / (Ni+Co+Mn)=0.005, F / (Ni+Co+Mn)=0.02.

[0239] Embodiment 14

[0240] The difference between this embodiment and embodiment 2 is that the raw materials in step (1) are different.

[0241] The nickel-cobalt-manganese precursor is nickel-cobalt-manganese hydroxide Ni 0.3 Co 0.1 Mn 0.6 (OH)2;

[0242] The lithium salt is lithium carbonate, and the molar ratio of each element satisfies: Li / (Ni+Co+Mn)=1.22;

[0243] The sodium salt is sodium carbonate, and the molar ratio of each element satisfies: Na / (Ni+Co+Mn)=0.23;

[0244] The dopants are Nb2O5 and NH4F, and the molar ratio of each element satisfies: Nb / (Ni+Co+Mn)=0.01, F / (Ni+Co+Mn)=0.02.

[0245] Embodiment 15

[0246] The difference between this embodiment and embodiment 2 is that the water washing time is 15 minutes.

[0247] Comparative Example 1

[0248] The difference between this comparative example and Example 2 is that the double alkali metal manganese-rich oxide is not coated with polyalkali metal phosphate, that is, step (4) is modified as follows:

[0249] The double alkali metal manganese-rich oxide is heated from room temperature to 500°C at a heating rate of 5°C / min and kept warm for 10 hours for a second sintering treatment; it is naturally cooled to room temperature in the furnace and passed through a 300-mesh sieve to obtain a modified lithium-rich manganese-based material.

[0250] Comparative Example 2

[0251] The difference between this comparative example and Example 2 is that the mass ratio of the double alkali metal manganese-rich oxide to the polyalkali metal phosphate is 100:3.

[0252] Comparative Example 3

[0253] The difference between this comparative example and Example 2 is that the raw materials in step (1) are different.

[0254] The nickel-cobalt-manganese precursor is nickel-cobalt-manganese hydroxide Ni 0.2 Mn 0.8 (OH)2;

[0255] The lithium salt is lithium carbonate, and the molar ratio of each element satisfies: Li / (Ni+Co+Mn)=1.49;

[0256] The sodium salt is sodium carbonate, and the molar ratio of each element satisfies: Na / (Ni+Co+Mn)=0.3;

[0257] The dopants are Nb2O5 and NH4F, and the molar ratio of each element satisfies: Nb / (Ni+Co+Mn)=0.005, F / (Ni+Co+Mn)=0.02.

[0258] Comparative Example 4

[0259] The difference between this comparative example and Example 2 is that the raw materials in step (1) are different.

[0260] The nickel-cobalt-manganese precursor is nickel-cobalt-manganese hydroxide Ni 0.45 Mn 0.55 (OH)2;

[0261] The lithium salt is lithium carbonate, and the molar ratio of each element satisfies: Li / (Ni+Co+Mn)=1.09;

[0262] The sodium salt is sodium carbonate, and the molar ratio of each element satisfies: Na / (Ni+Co+Mn)=0.19;

[0263] The dopants are Nb2O5 and NH4F, and the molar ratio of each element satisfies: Nb / (Ni+Co+Mn)=0.005, F / (Ni+Co+Mn)=0.02.

[0264] Comparative Example 5

[0265] The difference between this comparative example and Example 2 is that the raw materials in step (1) are different.

[0266] The nickel-cobalt-manganese precursor is nickel-cobalt-manganese hydroxide Ni 0.33 Co 0.01 Mn 0.66 (OH)2;

[0267] The lithium salt is lithium carbonate, and the molar ratio of each element satisfies: Li / (Ni+Co+Mn)=1.25;

[0268] The sodium salt is sodium carbonate, and the molar ratio of each element satisfies: Na / (Ni+Co+Mn)=0.25;

[0269] The dopants are Nb2O5 and NH4F, and the molar ratio of each element satisfies: Nb / (Ni+Co+Mn)=0.06, F / (Ni+Co+Mn)=0.02.

[0270] Comparative Example 6

[0271] The difference between this comparative example and Example 2 is that the expression of the polyalkali metal phosphate is Li2NaV2(PO4)3.

[0272] Comparative Example 7

[0273] The difference between this comparative example and Example 2 is that the expression of the polyalkali metal phosphate is Li 1.7 NeK 0.3 V2(PO4)3.

[0274] Comparative Example 8

[0275] The difference between this comparative example and Example 2 is that the expression of the polyalkali metal phosphate is Li3V2(PO4)3.

[0276] Comparative Example 9

[0277] The difference between this comparative example and Example 2 is that the inner core does not contain Na, that is, the difference between this comparative example and Example 2 is that the raw materials of step (1) are different.

[0278] The nickel-cobalt-manganese precursor is nickel-cobalt-manganese hydroxide Ni 0.33 Co 0.01 Mn 0.66 (OH)2;

[0279] The lithium salt is lithium carbonate, and the molar ratio of each element satisfies: Li / (Ni+Co+Mn)=1.25;

[0280] The dopants are Nb2O5 and NH4F, and the molar ratio of each element satisfies: Nb / (Ni+Co+Mn)=0.06, F / (Ni+Co+Mn)=0.02.

[0281] Comparative Example 10

[0282] The difference between this comparative example and Example 2 is that the Na content in the core is too high, that is, the difference between this comparative example and Example 2 is that the raw materials in step (1) are different.

[0283] The nickel-cobalt-manganese precursor is nickel-cobalt-manganese hydroxide Ni0.33 Co 0.01 Mn 0.66 (OH)2;

[0284] The lithium salt is lithium carbonate, and the molar ratio of each element satisfies: Li / (Ni+Co+Mn)=1.25;

[0285] The sodium salt is sodium carbonate, and the molar ratio of each element satisfies: Na / (Ni+Co+Mn)=0.35;

[0286] The dopants are Nb2O5 and NH4F, and the molar ratio of each element satisfies: Nb / (Ni+Co+Mn)=0.06, F / (Ni+Co+Mn)=0.02.

[0287] Comparative Example 11

[0288] The difference between this comparative example and Example 2 is that the core does not contain the R element, that is, the difference between this comparative example and Example 2 is that the raw materials of step (1) are different.

[0289] The nickel-cobalt-manganese precursor is nickel-cobalt-manganese hydroxide Ni 0.33 Co 0.01 Mn 0.66 (OH)2;

[0290] The lithium salt is lithium carbonate, and the molar ratio of each element satisfies: Li / (Ni+Co+Mn)=1.25;

[0291] The sodium salt is sodium carbonate, and the molar ratio of each element satisfies: Na / (Ni+Co+Mn)=0.25;

[0292] The dopant is NH4F, and the molar ratio of each element satisfies: F / (Ni+Co+Mn)=0.02.

[0293] Test Case

[0294] The modified lithium-rich manganese-based material was tested as follows:

[0295] (1) Morphology test: The modified lithium-rich manganese-based material of Example 2 was tested using a scanning electron microscope (SEM) of Hitachi, Japan. The results are shown in Figure 1 .

[0296] like Figure 1 As shown, the material surface has an obvious island structure, and the island structure is evenly coated on the material surface, and the particle size of the coating of the island structure is less than 1 μm.

[0297] (2) Composition test: X-ray powder diffraction (XRD) test was performed on the modified lithium-rich manganese-based materials of Examples 1-2 and Comparative Example 1. The results are shown in Figure 2 .

[0298] like Figure 2 As shown, there is no significant difference in the XRD spectra of the modified lithium-rich manganese-based materials of Examples 1-2 and Comparative Example 1. There is a crystal plane diffraction peak belonging to the P2 phase characteristics at a diffraction angle of 15.5°-16.1°, indicating that Na + The introduction of makes the core form a P2 type composite phase, which also shows that the cores of the three are basically the same, and the difference in their electrochemical performance mainly comes from whether the ion conductor layer coats the core. The XRD spectrum of the modified lithium-rich manganese-based material in comparative example 9 does not show the characteristic peak of the P2 phase due to the lack of sodium, and forms an obvious spinel phase due to the lack of lithium due to insufficient lithium.

[0299] (3) Element content: measured by an Optima 7000 inductively coupled plasma atomic emission spectrometer (ICP-AES) from Perkin Elmer, USA. The results are shown in Table 2.

[0300] It can be seen from Table 2 that the P content and V content in the modified lithium-rich manganese-based materials of Examples 1 to 14 and Comparative Examples 1 to 8 are consistent with their corresponding coating amounts (i.e., the mass ratio of the core and the ion conductor layer), confirming that the modified lithium-rich manganese-based materials contain polyalkali metal phosphate.

[0301] (4) Electrochemical performance test: The modified lithium-rich manganese-based material was used as the positive electrode material to make the positive electrode sheet, which was then assembled into a 2032-type button cell for electrochemical performance testing.

[0302] Preparation of positive electrode sheet: Using modified lithium-rich manganese-based material as positive electrode material, the modified lithium-rich manganese-based material is evenly dispersed in a proper amount of N-methylpyrrolidone at a mass ratio of 90:5:5 to obtain positive electrode slurry; the positive electrode slurry is coated on aluminum foil, dried at 120°C, rolled, and punched to form a positive electrode sheet with a diameter of 13 mm. The loading amount of the modified lithium-rich manganese-based material in the positive electrode sheet is about 12 mg / cm 2 .

[0303] Assemble the battery: In an argon-filled glove box, a 2032-type button cell was assembled using a lithium sheet as the negative electrode, a polypropylene microporous membrane (Celgard2400) as the separator, and 1M LiPF6 / ethylene carbonate (EC) + dimethyl carbonate (DMC) as the electrolyte.

[0304] Electrochemical performance test: At 25°C, the following electrochemical performance tests were conducted on the 2032 button cell using the Xinwei battery test system: ① Charge and discharge tests were conducted at 0.2C to evaluate the initial charge and discharge specific capacity and initial coulombic efficiency of the positive electrode material; ② Cycled 100 times (100T) at 1C to evaluate the cycle performance of the material; ③ Charge and discharge tests were conducted at 0.2C, 0.33C, 0.5C, and 1C to evaluate the rate performance of the material. Among them, the battery's charge and discharge voltage window is 2.5V~4.55V, and the charge and discharge current density of 1C (1 times the rated capacity) is 230 mA / g. The test results are shown in Table 2 and Figure 3~Figure 6 As shown. Among them, Figure 3 The first charge and discharge curve of the battery corresponding to Example 1 at 0.2C; Figure 4 The first charge and discharge curve of the battery corresponding to Example 2 at 0.2C; Figure 5 The first charge and discharge curve of the battery corresponding to Comparative Example 1 at 0.2C; Figure 6 Graph showing the test results of the cycle stability of the batteries corresponding to Examples 1-2 and Comparative Example 1 at 1C.

[0305] It can be seen from Table 2 that compared with the uncoated comparative example 1, the discharge capacity, rate performance and cycle stability of the modified lithium-rich manganese-based materials of Examples 1 to 14 are significantly improved.

[0306] Examples 1 to 3 use different coating amounts (i.e., the mass ratio of the core to the ion conductor layer). As the coating amount increases, the electrochemical performance increases first and then decreases. When the mass ratio of the core to the ion conductor layer is 100:1, the improvement effect on the discharge capacity, rate performance, and cycle stability is most significant.

[0307] Taking Example 2 as a reference, part of the V element in the ion conductor layer of Example 4 is replaced by Al element, and the electrochemical performance is reduced; the sintering temperature of Examples 5 and 6 during the second sintering treatment is different. The higher the sintering temperature, the better the discharge capacity and rate performance, but the cycle stability first increases and then decreases. The molar ratio of Li and Na in the ion conductor layer of Examples 7 and 8 is different. As the Li content decreases and the Na content increases, the discharge capacity and rate performance gradually decrease, but the cycle stability first increases and then decreases; the types and doping amounts of R elements in the cores of Examples 9 to 14 are different, resulting in different effects on improving the electrochemical performance; the water washing time of the intermediate in Example 15 is extended to 15 minutes, which has little effect on the electrochemical performance, but the production efficiency is significantly reduced.

[0308] Taking Example 2 as a reference, the coating amount of Example 2 is too high, and the doping amount of the Nb element of Example 5 is too high, both of which will lead to a decrease in discharge capacity. Although no doping elements are used in Example 11, the capacity only decreases slightly, but the cycle stability is significantly deteriorated.

[0309] It can be seen from Example 2, Examples 9 to 13 and Comparative Examples 3 to 4 that if the Mn content is too high, the kinetics will decrease, and thus the discharge capacity and rate performance will decrease significantly; if the Mn content is too low, although the kinetics are improved, the lithium-rich phase and P2 phase are insufficient, resulting in a decrease in the first coulombic efficiency, a decrease in discharge capacity, and deterioration of the cycle stability.

[0310] Taking Example 2 as a reference, the ion conductor layer of Comparative Example 6 does not contain K + It has little effect on the discharge capacity and first coulombic efficiency of the material, but the cycle stability is greatly reduced. This is because the ion conductor layer will also undergo deep lithium / sodium desorption under high voltage and transform into V2(PO4)3 phase, which will seriously reduce the ion / electronic conductivity and cause the ion conductor layer to fail, which in turn increases polarization.

[0311] Taking Example 2 as a reference, the K + The ion content is high due to K + The ionic radius is large and does not participate in electrochemical deintercalation, resulting in some lithium / sodium ions being unable to be intercalated back during the first discharge process, and the lithium / sodium ion diffusion channels are relatively reduced. Therefore, the discharge capacity and rate performance are reduced, but the cycle stability is still high.

[0312] It can be seen from Example 2 and Comparative Examples 6 to 8 that the ion conductor layer of Comparative Example 8 contains only Li + An alkali metal element, the material's cycle performance and rate performance are both reduced. This is because the radius of the Li+ ion is smaller, and the lattice formed by the ion conductor layer itself during the sintering process will be smaller than that of the Na-containing + or K + The lattice of the sintered phase is smaller, so it will hinder the Na ions with larger ions radius from the inner core. + diffusion.

[0313] Taking Example 2 as a reference, since no sodium is added to the core of Comparative Example 9, the capacity of the material is extremely low, which is consistent with the result that there is no P2 characteristic peak in its XRD spectrum and there is an obvious spinel phase; while Comparative Example 10 adds excessive sodium, although it does not affect the capacity of the material, the excessive sodium content increases the specific surface area and residual alkali, resulting in deterioration of the cycle stability.

[0314] Table 1. Related parameters of modified lithium-rich manganese-based materials

[0315]

[0316]

[0317] Table 2. Performance comparison of modified lithium-rich manganese-based materials

[0318]

[0319] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0320] The above-described embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of protection of the present application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the scope of protection of the present application. Therefore, the scope of protection of the present application shall be subject to the attached claims.

Claims

1. A modified lithium-rich manganese-based material, characterized in that: It comprises a core and an ion conductor layer covering the core, wherein the mass ratio of the core to the ion conductor layer is 100:(0.05-2); The inner core includes a double alkali metal manganese-rich oxide, and the expression of the double alkali metal manganese-rich oxide is: Li a Na b Ni x Co y Mn z R 1-x-y-z O c X d ; Among them, 1.1 <a<1.5,0.03<b≤0.3,0≤d≤0.1,a+b+1=c+d; 0.25≤x≤0.4, 0≤y≤0.1, 0.6≤z≤0.75, 0<1-xyz≤0.05; The R element includes one or more of Ca, Al, Ba, Ce, Cr, Cu, Fe, K, La, Mg, Mo, Te, Nb, Sb, Sm, Ta, Ti, V, W, Y, Sn, Zn and Zr; The X element includes one or more of F, Cl and S; The ion conductor layer includes a polyalkali metal phosphate, and the polyalkali metal phosphate is expressed as: Li e Na f K h M2(PO4)3; Among them, 0.5≤e≤2.3, 0.5≤f≤2.3, 0 <h≤0.2,e+f+h=3; The M element includes one or more of Al, V, Cr, La and Y.

2. The modified lithium-rich manganese-based material according to claim 1, characterized in that: The R element includes one or more of Nb, W, Mo, Sb, Cr and Zr.

3. The modified lithium-rich manganese-based material according to claim 1, characterized in that: The M element includes one or more of V and Al.

4. The modified lithium-rich manganese-based material according to any one of claims 1 to 3, characterized in that: The modified lithium-rich manganese-based material meets one or more of the following conditions: (1) The thickness of the ion conductor layer is 5 nm to 20 nm; (2) The ion conductor layer partially covers the core, and the ion conductor layer is supported on a portion of the surface of the core to form a dispersed island structure, and the median particle size of each of the island structures is less than 1 μm; (3) The median particle size of the modified lithium-rich manganese-based material is 2 μm to 15 μm.

5. A method for preparing a modified lithium-rich manganese-based material, characterized in that: The following steps are involved: Mixing a double alkali metal manganese-rich oxide and a polyalkali metal phosphate, and performing a second sintering treatment so that the polyalkali metal phosphate covers the double alkali metal manganese-rich oxide; The mass ratio of the double alkali metal manganese-rich oxide to the polyalkali metal phosphate is 100:(0.05-2); The double alkali metal manganese-rich oxide is expressed as: Li a Na b Ni x Co y Mn z R 1-x-y-z O c X d ; Among them, 1.1 <a<1.5,0.03<b≤0.3,0≤d≤0.1,a+b+1=c+d; 0.25≤x≤0.4, 0≤y≤0.1, 0.6≤z≤0.75, 0<1-xyz≤0.05; The R element includes one or more of Ca, Al, Ba, Ce, Cr, Cu, Fe, K, La, Mg, Mo, Te, Nb, Sb, Sm, Ta, Ti, V, W, Y, Sn, Zn and Zr; The X element includes one or more of F, Cl and S; The polyalkali metal phosphate is expressed as: Li e Na f K h M2(PO4)3; Among them, 0.5≤e≤2.3, 0.5≤f≤2.3, 0 <h≤0.2,e+f+h=3; The M element includes one or more of Al, V, Cr, La and Y.

6. The method for preparing the modified lithium-rich manganese-based material according to claim 5, characterized in that: One or more of the following conditions are met: (1) The R element includes one or more of Nb, W, Mo, Sb, Cr and Zr; (2) The M element includes one or more of V and Al.

7. The method for preparing the modified lithium-rich manganese-based material according to claim 5, characterized in that: The second sintering process comprises the following steps: Keep warm at 300℃~800℃ for 3h~15h.

8. The method for preparing the modified lithium-rich manganese-based material according to any one of claims 5 to 7, characterized in that: The preparation method of the double alkali metal manganese-rich oxide comprises the following steps: Mixing a nickel-cobalt-manganese precursor, a lithium salt, a sodium salt and a dopant, and performing a first sintering treatment to prepare an intermediate; washing and drying the intermediate to prepare the double alkali metal manganese-rich oxide; Wherein, the dopant includes an R source, or the dopant includes an R source and an X source.

9. The method for preparing the modified lithium-rich manganese-based material according to claim 8, characterized in that: One or more of the following conditions are met: (1) The nickel-cobalt-manganese precursor includes one or more of oxides, hydroxides, carbonates, oxalates and ethanolates containing nickel, cobalt and manganese elements; (2) The lithium salt includes one or more of lithium carbonate, lithium hydroxide, lithium nitrate, lithium sulfate, lithium chloride and lithium fluoride; (3) The sodium salt includes one or more of sodium carbonate, sodium hydroxide, sodium sulfate, sodium oxalate, sodium acetate, sodium chloride and sodium fluoride; (4) The R source includes one or more of oxides, fluorides, hydroxides and ethanolates containing the R element; (5) The X source includes one or more of fluoride, chloride and sulfide.

10. The method for preparing the modified lithium-rich manganese-based material according to claim 8, characterized in that: The first sintering process comprises the following steps: Keep warm at 300℃~800℃ for 0h~10h, and keep warm at 800℃~1000℃ for 4h~20h.

11. The method for preparing the modified lithium-rich manganese-based material according to claim 8, characterized in that: The washing process comprises the following steps: Wash with water at a temperature of 0℃~25℃ for 1min~10min, and dehydrate.

12. A positive electrode material, characterized in that: The modified lithium-rich manganese-based material is made from the modified lithium-rich manganese-based material as described in any one of claims 1 to 4, or is made from the modified lithium-rich manganese-based material prepared by the preparation method of the modified lithium-rich manganese-based material as described in any one of claims 5 to 11.

13. A positive electrode sheet, characterized in that: It comprises a positive electrode current collector and a positive electrode active layer covering the positive electrode current collector, wherein the positive electrode active layer comprises the positive electrode material as claimed in claim 12.

14. A lithium ion battery, characterized in that: Comprising the positive electrode sheet as claimed in claim 13.

Citation Information

Patent Citations

  • Fast ion conductor coated metal doped modified lithium-rich cobalt-free single crystal material and preparation method thereof

    CN115198342A

  • NASICON type solid electrolyte, positive electrode material coated by same and preparation method of NASICON type solid electrolyte

    CN116789094A