Biomass-based self-supporting hard carbon negative electrode material and preparation method thereof

Through the preparation method of biomass-based self-supported hard carbon material, the problems of low efficiency and complex preparation of hard carbon anode material are solved, and cost reduction and performance improvement are achieved, which are suitable for high-efficiency energy density applications of sodium ion batteries.

CN118929627AActive Publication Date: 2024-11-12XIAN UNIV OF TECH

Patent Information

Application Number
CN202411006182.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

The existing hard carbon anode material has low efficiency, complex production and high cost problems, especially in sodium ion batteries, which are slow in kinetics and short cycle life.

Method used

The preparation method of biomass-based self-supported hard carbon negative electrode material is adopted. The biomass is treated by a mixed solution of acid solution and hydrogen peroxide, and the solvent-thermal reaction and ultrasonic dispersion are carried out. After forming a pre-carbonized film, it is carbonized at high temperature under an inert atmosphere. It is constructed from the construction of the Support hard carbon materials to avoid the addition of binders and conductive carbon black.

Benefits of technology

It improves the first Coulomb efficiency of hard carbon materials, reduces production costs, enhances conductivity, improves the performance and energy density of sodium ion batteries, simplifies the preparation process, and is suitable for large-scale production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118929627A_ABST
    Figure CN118929627A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a biomass-based self-supporting hard carbon negative electrode material, which comprises the following steps: preparing a mixed solution of an acid solution and hydrogen peroxide, and fully stirring to obtain a mixed solution; soaking biomass in the mixed solution according to a certain proportion, and then carrying out solvothermal reaction to obtain a biomass precursor; ultrasonically dispersing the biomass precursor in a solvent, and then performing suction filtration to obtain a biomass film; carrying out pre-carbonization treatment on the biomass film to obtain a pre-carbonized film; and performing high-temperature carbonization on the pre-carbonized film in an inert atmosphere to obtain the self-supporting hard carbon negative electrode material. According to the invention, the self-supporting hard carbon material is constructed by virtue of the characteristics of the biomass, a binder, conductive carbon black and a current collector are not needed, the influence of additional additives is avoided, the production cost of the sodium ion battery is saved, meanwhile, the sodium storage performance of the battery is improved, and the obtained self-supporting hard carbon negative electrode material has excellent sodium storage capacity and high first coulombic efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of methods for preparing carbon-based electrode materials for sodium ion batteries, and specifically relates to methods for preparing biomass-based self-supporting hard carbon negative electrode materials; it also relates to biomass-based self-supporting hard carbon negative electrode materials. Background Art

[0002] With the acceleration of the commercialization of lithium-ion batteries, the huge demand for lithium resources has forced the production cost of lithium-ion batteries to rise sharply. In order to meet the growing demand for energy storage and power systems, it is urgent to explore other rechargeable secondary batteries. Sodium-ion batteries have attracted widespread attention from researchers due to their similar physical properties to lithium and abundant sodium resources. However, compared with lithium ions, the larger ionic radius of sodium ions usually leads to slow kinetics and shorter cycle life. To this end, in-depth exploration of the composition of sodium-ion batteries and the development of new electrode materials are the key to solving the above problems.

[0003] Hard carbon is composed of randomly dispersed graphene layers, which provides a large number of sodium accessible sites and therefore has a high theoretical sodium storage capacity. In addition to its low working potential and abundant raw material resources, hard carbon is the most promising negative electrode material for high energy density sodium ion batteries (SIBs). So far, common hard carbon materials are mainly powder materials. For example, patent CN118183741 A reports a coal-based hard carbon negative electrode material for sodium electricity, a preparation method thereof, and a sodium ion battery. The process mainly includes blending coal and carboxylate, pre-carbonizing and carbonizing to obtain a coal-based hard carbon negative electrode material for sodium electricity. Patent CN118005003B discloses an ultra-microporous hard carbon material, a preparation method, and an application thereof. The process mainly includes heat treating a phenolic resin and a curing agent, pre-carbonizing, annealing, and carbonizing to obtain a hard carbon material. However, powder materials often need to be combined with binders and conductive carbon black to make electrodes. The addition of binders and conductive carbon black will not only increase the production cost of sodium-ion batteries, but also the binder itself is not conductive and the conductive carbon black has a large specific surface area, which will affect the sodium storage performance of hard carbon materials.

[0004] Therefore, in order to save costs and reduce energy consumption, the key to improving the electrochemical properties of hard carbon materials is to design the structure of hard carbon materials and construct an integrated self-supporting hard carbon structure. Summary of the invention

[0005] The purpose of the present invention is to provide a method for preparing a biomass-based self-supporting hard carbon negative electrode material, so as to solve the problems of low first coulombic efficiency, complex preparation and high cost of existing hard carbon negative electrode materials.

[0006] The present invention also aims to provide a biomass-based self-supporting hard carbon negative electrode material.

[0007] The first technical solution adopted by the present invention is a method for preparing a biomass-based self-supporting hard carbon negative electrode material, and the specific operation steps are as follows:

[0008] Step 1, preparing an acidic solution and a hydrogen peroxide mixed solution, and fully stirring the solution to obtain a mixed solution;

[0009] Step 2, soaking the biomass in the mixed solution, and then performing a solvothermal reaction to obtain a biomass precursor;

[0010] Step 3, ultrasonically dispersing the biomass precursor in a solvent, and then filtering to obtain a biomass film;

[0011] Step 4, pre-carbonizing the biomass film to obtain a pre-carbonized film;

[0012] Step 5: Carbonize the pre-carbonized film at high temperature under an inert atmosphere to obtain a self-supporting hard carbon negative electrode material.

[0013] The present invention is also characterized in that:

[0014] In step 1, the mass ratio of the acidic solution to hydrogen peroxide is 1:0.05-0.5.

[0015] In step 2, the biomass includes one or more of straw, basswood, pinewood, buckwheat husk, apricot husk, and coconut husk.

[0016] In step 2, the mass ratio of biomass to mixed solution is 1:5-50.

[0017] In step 2, the temperature of the solvent thermal reaction is 100 to 150° C., and the reaction time is 1 to 10 hours.

[0018] In step 3, the selected solvent includes one or more of deionized water, ethanol, isopropanol, and NN dimethylformamide.

[0019] In step 4, the pre-carbonization temperature is 200-260°C and the time is 0.5-5h.

[0020] In step 5, the inert atmosphere is nitrogen or argon.

[0021] In step 5, the heating rate is 0.5-8°C / min, the calcination time is 1-12h, and the constant temperature is 900-1700°C.

[0022] The second technical solution adopted by the present invention is: the self-supporting hard carbon negative electrode material obtained by the preparation method of the biomass-based self-supporting hard carbon negative electrode material of the present invention, and the application of the self-supporting hard carbon material as the negative electrode material in a sodium ion battery.

[0023] The beneficial effects of the present invention are:

[0024] (1) The hard carbon of the present invention uses biomass as a precursor, reforms the biomass microstructure by solvent pretreatment, and obtains a self-supporting hard carbon negative electrode material by combining solvent thermal reaction, simple filtration and carbonization process. In the solvent thermal reaction, the acidic solution and hydrogen peroxide can remove the hemicellulose and lignin of the biomass itself, thereby retaining the cellulose with relatively complete crystallinity, purifying the chemical composition of the biomass and helping to unify the biomass microstructure. Further, by constructing a self-supporting hard carbon film, on the one hand, the addition of binders and conductive carbon black is avoided, saving the production cost of hard carbon materials. On the other hand, due to its own interconnected network structure and the absence of foreign substances, the conductivity of the material is enhanced. At the same time, side reactions are avoided, the first coulomb efficiency of the hard carbon material is improved, and the performance of sodium ion batteries is improved.

[0025] (2) The preparation method of the present invention is simple and convenient, and can be used to quickly and large-scale produce hard carbon materials with excellent performance, which is beneficial to improving the energy density of sodium-ion full batteries and helps promote the development of the sodium-ion battery industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is a SEM image of the self-supporting hard carbon negative electrode material prepared in Example 1 of the present invention.

[0027] Figure 2 This is the XRD pattern of the self-supporting hard carbon negative electrode material prepared in Example 1 of the present invention.

[0028] Figure 3 This is an X-ray photoelectron spectrum of the self-supporting hard carbon negative electrode material prepared in Example 1 of the present invention.

[0029] Figure 4 This is a charge and discharge curve diagram of the self-supporting hard carbon negative electrode material prepared in Example 1 of the present invention.

[0030] Figure 5 This is the cycle performance curve of the self-supporting hard carbon negative electrode material prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0031] In order to further understand the present invention, the present invention is described below in conjunction with embodiments. These descriptions are only to further explain the features and advantages of the present invention and are not intended to limit the claims of the present invention.

[0032] Example 1

[0033] A mixed solution of sulfonic acid and hydrogen peroxide is prepared in a mass ratio of 1:0.1, and it is fully stirred to obtain a mixed solution; then, pine wood is immersed in the mixed solution in a mass ratio of 1:10, and a solvent thermal reaction is carried out at a reaction temperature of 100°C for 8 hours to obtain a biomass precursor; the biomass precursor is ultrasonically dispersed in an ethanol solution, and then filtered to obtain a biomass film; the biomass film is pre-carbonized at a constant temperature of 230°C for 2 hours to obtain a pre-carbonized film; the pre-carbonized film is carbonized at a high temperature in a nitrogen atmosphere at a carbonization rate of 2°C / min, a constant temperature of 1300°C, and a calcination time of 5 hours to obtain a self-supporting hard carbon negative electrode material.

[0034] Figure 1 The SEM image of the self-supporting hard carbon negative electrode material prepared in Example 1 of the present invention shows that the self-supporting hard carbon material is composed of ribbon-like fibers of varying lengths, with a bandwidth of about 40 microns. This is because after the biomass is pretreated, hemicellulose, lignin, starch and other substances with low content and easy to decompose are decomposed, leaving only cellulose with higher crystallinity, thereby forming a self-supporting structure through self-assembly.

[0035] Figure 2 This is the XRD diagram of the self-supporting hard carbon negative electrode material prepared in Example 1 of the present invention. It can be seen from the figure that the self-supporting hard carbon has typical amorphous carbon characteristics, indicating that the material belongs to hard carbon material. At the same time, the graphite layer spacing of the hard carbon calculated by the Scherrer formula is about 3.9nm, which is larger than the sodium ion radius, so that the sodium ions can be effectively embedded / extracted.

[0036] Figure 3 This is an X-ray photoelectron spectrum of the self-supporting hard carbon negative electrode material prepared in Example 1 of the present invention. From the figure, it can be seen that the self-supporting hard carbon material contains only carbon and oxygen, and no other impurities.

[0037] The self-supporting hard carbon negative electrode material obtained in Example 1 was used as the working electrode and metallic sodium was used as the counter electrode to assemble a button cell and test its charge and discharge performance. Figure 4 As shown, at a current density of 30 mA / g, the first charge capacity is 274.7 mAh / g, the first discharge capacity is 296.8 mAh / g, and the first coulombic efficiency reaches 92.5%.

[0038] Figure 5 This is a cycle performance diagram of the self-supporting hard carbon negative electrode material prepared in Example 1 of the present invention. At 200 mA / g, after 100 cycles, its reversible capacity can be maintained at 230 mAh / g.

[0039] Example 2

[0040] A mixed solution of sulfonic acid and hydrogen peroxide is prepared in a mass ratio of 1:0.2, and it is fully stirred to obtain a mixed solution; then, pine wood is immersed in the mixed solution in a mass ratio of 1:5, and a solvent thermal reaction is carried out at a reaction temperature of 120°C for 10 hours to obtain a biomass precursor; the biomass precursor is ultrasonically dispersed in an ethanol solution, and then filtered to obtain a biomass film; the biomass film is pre-carbonized at a constant temperature of 200°C for 4 hours to obtain a pre-carbonized film; the pre-carbonized film is high-temperature carbonized in a nitrogen atmosphere at a carbonization rate of 1°C / min, a constant temperature of 1300°C, and a calcination time of 5 hours to obtain a self-supporting hard carbon negative electrode material.

[0041] Example 3

[0042] A mixed solution of acetic acid and hydrogen peroxide is prepared in a mass ratio of 1:0.2, and it is fully stirred to obtain a mixed solution; then, the straw is immersed in the mixed solution in a mass ratio of 1:8, and a solvent thermal reaction is carried out at a reaction temperature of 130°C for 6 hours to obtain a biomass precursor; the biomass precursor is ultrasonically dispersed in deionized water, and then filtered to obtain a biomass film; the biomass film is pre-carbonized at a constant temperature of 250°C for 3 hours to obtain a pre-carbonized film; the pre-carbonized film is high-temperature carbonized in a nitrogen atmosphere at a carbonization rate of 3°C / min, a constant temperature of 1300°C, and a calcination time of 5 hours to obtain a self-supporting hard carbon negative electrode material.

[0043] Example 4

[0044] A mixed solution of hypochlorous acid and hydrogen peroxide is prepared in a mass ratio of 1:0.3, and it is fully stirred to obtain a mixed solution; then, balsa wood is immersed in the mixed solution in a mass ratio of 1:10, and a solvent thermal reaction is carried out at a reaction temperature of 120°C for 10 hours to obtain a biomass precursor; the biomass precursor is ultrasonically dispersed in an ethanol solution, and then filtered to obtain a biomass film; the biomass film is pre-carbonized at a constant temperature of 220°C for 1 hour to obtain a pre-carbonized film; the pre-carbonized film is high-temperature carbonized in a nitrogen atmosphere at a carbonization rate of 2°C / min, a constant temperature of 1300°C, and a calcination time of 5 hours to obtain a self-supporting hard carbon negative electrode material.

[0045] Example 5

[0046] A mixed solution of formic acid and hydrogen peroxide was prepared in a mass ratio of 1:0.3, and it was fully stirred to obtain a mixed solution; then, buckwheat husks were immersed in the mixed solution in a mass ratio of 1:5, and a solvothermal reaction was carried out at a reaction temperature of 120°C for 10 hours to obtain a biomass precursor; the biomass precursor was ultrasonically dispersed in an ethanol solution, and then filtered to obtain a biomass film; the biomass film was pre-carbonized at a constant temperature of 230°C for 2 hours to obtain a pre-carbonized film; the pre-carbonized film was high-temperature carbonized in a nitrogen atmosphere at a carbonization rate of 2°C / min, a constant temperature of 1300°C, and a calcination time of 5 hours to obtain a self-supporting hard carbon negative electrode material.

[0047] Example 6

[0048] A mixed solution of sulfonic acid and hydrogen peroxide is prepared in a mass ratio of 1:0.2, and it is fully stirred to obtain a mixed solution; then, apricot shells are immersed in the mixed solution in a mass ratio of 1:5, and a solvent thermal reaction is carried out at a reaction temperature of 120°C for 10 hours to obtain a biomass precursor; the biomass precursor is ultrasonically dispersed in an ethanol solution, and then filtered to obtain a biomass film; the biomass film is pre-carbonized at a constant temperature of 230°C for 2 hours to obtain a pre-carbonized film; the pre-carbonized film is high-temperature carbonized in a nitrogen atmosphere at a carbonization rate of 0.5°C / min, a constant temperature of 1700°C, and a calcination time of 5 hours to obtain a self-supporting hard carbon negative electrode material.

[0049] Example 7

[0050] A mixed solution of sulfonic acid and hydrogen peroxide is prepared in a mass ratio of 1:0.2, and it is fully stirred to obtain a mixed solution; then, pine wood is immersed in the mixed solution in a mass ratio of 1:5, and a solvent thermal reaction is carried out at a reaction temperature of 120°C for 10 hours to obtain a biomass precursor; the biomass precursor is ultrasonically dispersed in an ethanol solution, and then filtered to obtain a biomass film; the biomass film is pre-carbonized at a constant temperature of 230°C for 2 hours to obtain a pre-carbonized film; the pre-carbonized film is high-temperature carbonized in a nitrogen atmosphere at a carbonization rate of 1°C / min, a constant temperature of 1500°C, and a calcination time of 5 hours to obtain a self-supporting hard carbon negative electrode material.

[0051] Example 8

[0052] A mixed solution of sulfonic acid and hydrogen peroxide is prepared in a mass ratio of 1:0.2, and it is fully stirred to obtain a mixed solution; then, pine wood is immersed in the mixed solution in a mass ratio of 1:5, and a solvent thermal reaction is carried out at a reaction temperature of 120°C for 10 hours to obtain a biomass precursor; the biomass precursor is ultrasonically dispersed in an ethanol solution, and then filtered to obtain a biomass film; the biomass film is pre-carbonized at a constant temperature of 230°C for 2 hours to obtain a pre-carbonized film; the pre-carbonized film is high-temperature carbonized in a nitrogen atmosphere at a carbonization rate of 1°C / min, a constant temperature of 1100°C, and a calcination time of 5 hours to obtain a self-supporting hard carbon negative electrode material.

[0053] Comparative Example 1

[0054] The difference from Example 1 is that the amount of hydrogen peroxide added is 0, and the acidic solution is acetic acid. The rest is the same as Example 1 and will not be repeated here.

[0055] Comparative Example 2

[0056] The difference from Example 1 is that the amount of hydrogen peroxide added is 0, and the acidic solution is oxalic acid. The rest is the same as Example 1 and will not be repeated here.

[0057] The above test results are shown in Table 1.

[0058] Table 1

[0059] Discharge specific capacity (mAh / g) First effect (%) Example 1 296.8 92.5 Example 2 267.3 91.2 Example 3 278.5 90.6 Example 4 271.4 88.5 Example 5 259.8 89.1 Example 6 229.5 90.5 Example 7 238.7 91.7 Example 8 248.4 88.9 Comparative Example 1 232.8 83.2 Comparative Example 2 240.7 84.1

[0060] It can be seen from Example 1 and Examples 6-8 that if the carbonization temperature is too high, the pores of the carbon material shrink, and the sodium ions cannot be effectively embedded to generate capacity, resulting in a decrease in the specific capacity of the obtained material.

[0061] It can be seen from Example 1 and Comparative Examples 1-2 that without the addition of hydrogen peroxide, substances such as hemicellulose, lignin and starch in the biomass cannot be effectively removed, affecting the microstructure of the material. At the same time, there are a large number of oxygen-containing groups in the above substances, which are difficult to effectively remove through carbonization, thereby affecting the specific capacity and first coulombic efficiency of the self-supporting hard carbon negative electrode material.

[0062] Analysis of the key innovative points of the present invention:

[0063] From the above data, it can be seen that the present invention adopts a solvothermal method to decompose hemicellulose, lignin, starch and other substances in the biomass with the help of acid and hydrogen peroxide, accurately adjust the biomass structure, and obtain ribbon cellulose. By taking advantage of its structural advantages, a self-supporting material can be formed by simple filtration. The self-supporting structure formed can show excellent first coulomb efficiency. At the same time, the performance of the obtained material varies according to the different treatment conditions, indicating that the process conditions need to be precisely controlled to improve the capacity and first coulomb efficiency of the self-supporting hard carbon negative electrode material of the present invention.

[0064] Feasibility analysis of lignin removal: Hydrogen peroxide (H2O2) as an environmentally friendly chemical can effectively remove lignin, producing only oxygen and water during the reaction process. – , O 2- and HO are easily formed. Among these anions and free radicals, HOO – ions react with lignin as the main reactive group, cleaving the bonds between the aromatic rings and side chains of lignin. – Further destroy the carbonyl and olefin aldehyde structures in the side chains of lignin molecules, thereby forming ethylene oxide intermediates, which are further depolymerized into small molecular aliphatic compounds. – The ion reaction mechanism is similar, HO – Ions, HO and O 2- Free radicals also contribute to the oxidation, hydrolysis and degradation of lignin, thereby achieving the dissociation of the hard components of the wood cell wall.

[0065] Feasibility analysis of hemicellulose removal: Hemicellulose is mainly carbohydrates. During the autohydrolysis process, H2O molecules dissociate at high temperature to produce protons, while in acidic solution hydrolysis, the added acid dissociates and diffuses through the bulk solution to the molecular pores to reach the reaction site; these protons catalyze the cleavage of acetyl groups in hemicellulose to form weak acids, exacerbating the decomposition of hemicellulose.

[0066] Theoretical feasibility of preparing biomass films:

[0067] In natural wood, lignin's rich functional groups and amorphous network structure make it an important filler and adhesive, which enhances the mechanical strength and stiffness of the wood structure by cross-linking with carbohydrates (cellulose, hemicellulose) in the cell wall. Delignification can achieve the shrinkage and dissociation of the cell wall of the wooden structure, thereby stripping off cellulose and hemicellulose. Cellulose and hemicellulose are essentially carbohydrates, and acidic solutions can further decompose the short-chain polymers and amorphous tissues in the two into furan derivatives, phenolic compounds and other substances, promoting the decomposition and stripping of the cell wall framework structure and the formation of two-dimensional cellulose nanosheets. Based on the flexible characteristics of cellulose itself and the properties of two-dimensional materials, the construction of flexible biomass carbon films can be completed by simple filtration and carbonization. Self-supporting materials can circumvent the use of conductive agents, binders and current collectors in traditional processes, significantly reducing the volume and mass of batteries, while improving their energy density and power density.

[0068] The above is only a preferred specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto, that is, it does not mean that the present invention must rely on the above process steps to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the raw materials selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.

Claims

1. A method for preparing a biomass-based self-supporting hard carbon negative electrode material, characterized in that: The specific steps are as follows: Step 1, preparing an acidic solution and a hydrogen peroxide mixed solution, and fully stirring the solution to obtain a mixed solution; Step 2, soaking the biomass in the mixed solution, and then performing a solvothermal reaction to obtain a biomass precursor; Step 3, ultrasonically dispersing the biomass precursor in a solvent, and then filtering to obtain a biomass film; Step 4, pre-carbonizing the biomass film to obtain a pre-carbonized film; Step 5: Carbonize the pre-carbonized film at high temperature under an inert atmosphere to obtain a self-supporting hard carbon negative electrode material.

2. The method for preparing a biomass-based self-supporting hard carbon negative electrode material according to claim 1, characterized in that: In step 1, the acidic solution includes one or more of formic acid, sulfinic acid, oxalic acid, hypochlorous acid, acetic acid, nitrous acid, citric acid, and benzoic acid.

3. The method for preparing a biomass-based self-supporting hard carbon negative electrode material according to claim 1, characterized in that: The mass ratio of the acidic solution to hydrogen peroxide in step 1 is 1:0.05-0.

5.

4. The method for preparing a biomass-based self-supporting hard carbon negative electrode material according to claim 1, characterized in that: In step 2, the biomass includes one or more of straw, basswood, pinewood, buckwheat husk, apricot husk, and coconut husk.

5. The method for preparing a biomass-based self-supporting hard carbon negative electrode material according to claim 1, characterized in that: In step 2, the mass ratio of the biomass to the mixed solution is 1:5-50; the temperature of the solvent thermal reaction is 100-150° C., and the reaction time is 1-10 hours.

6. The method for preparing a biomass-based self-supporting hard carbon negative electrode material according to claim 1, characterized in that: In step 3, the solvent includes one or more of deionized water, ethanol, isopropanol, and N-N-dimethylformamide.

7. The method for preparing a biomass-based self-supporting hard carbon negative electrode material according to claim 1, characterized in that: In step 4, the pre-carbonization temperature is 200-260° C. and the time is 0.5-5 h.

8. The method for preparing a biomass-based self-supporting hard carbon negative electrode material according to claim 1, characterized in that: In step 5, the inert atmosphere is nitrogen or argon.

9. The method for preparing a biomass-based self-supporting hard carbon negative electrode material according to claim 1, characterized in that: In step 5, the heating rate is 0.5-8°C / min, the calcination time is 1-12h, and the constant temperature is 900-1700°C.

10. A biomass-based self-supporting hard carbon negative electrode material obtained by the preparation method according to any one of claims 1 to 9, wherein the biomass-based self-supporting hard carbon negative electrode material is used in a sodium ion battery.

Citation Information

Patent Citations

  • Preparation method of porous graphene active carbon material as well as product and application thereof

    CN107555424A

  • Preparation methods for high capacity biomass hard carbon anode material of sodium ion battery

    CN109921018A

  • Waste biomass kernel derived hard carbon material as well as preparation method and application thereof

    CN115863634A

  • High-performance lamellar hard carbon and preparation method thereof

    CN116102000A

  • Preparation method and application of biomass hard carbon sodium ion battery negative electrode material

    CN117246997A

Cited By

  • Self-supporting membrane negative electrode material, preparation method thereof and sodium ion battery

    CN119812204A

  • Preparation method of high-magnification biomass hard carbon composite film material

    CN121035187A