A high-flexibility optical film material for polarizer and preparation method thereof
Through stearic acid modification and grafting of alkenyl groups, the flexibility of the TCA optical film is improved, solving the problem of fragility of the pure TCA film, achieving a combination of high flexibility and excellent optical properties, and is suitable for the application of polarizers.
Patent Information
- Application Number
- CN202411030319.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-07-30
AI Technical Summary
Pure TCA optical films lack sufficient flexibility, limiting their use in applications requiring high flexibility. At the same time, existing methods may affect the optical properties of the film by adding plasticizers or composite polymers.
By modifying cellulose with stearic acid, stearic acid-modified cellulose triacetate is prepared, and the terminal alkenyl group is grafted onto it to perform olefin polymerization to improve the flexibility and optical properties of the material.
It is possible to significantly improve the flexibility of the TCA optical film, enhance the tensile strength, crack resistance and wear resistance while ensuring the optical performance, and provide excellent mechanical properties and broad application prospects.
Smart Images

Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of optical materials, and in particular is a high-flexibility optical film material for polarizers and a preparation method thereof. Background Art
[0002] TCA (cellulose triacetate) optical film is mainly used as an optical film for manufacturing polarizers, especially in the production process of liquid crystal displays (LCDs), where it plays a vital role. It is widely used as a protective film and optical enhancement film for mobile phones, tablet computers, televisions, display screens, camera lenses and other products.
[0003] However, pure TCA optical film itself is relatively brittle and lacks sufficient flexibility, which limits its use in some applications that require high flexibility. The existing technology generally improves the flexibility of TCA optical film by adding plasticizers or compounding other polymers, but these methods may affect other optical properties of the film. Therefore, it is of great research significance to effectively improve the flexibility of TCA optical film by chemically modifying TCA while ensuring optical properties. Summary of the invention
[0004] To solve the above problems, an object of the present invention is to provide a highly flexible optical film material for polarizer and a preparation method thereof.
[0005] In order to achieve the above object, the present invention is implemented through the following technical solutions:
[0006] A highly flexible optical film material for polarizers is prepared according to the following method: cellulose is modified by stearic acid to obtain stearic acid-modified triacetyl cellulose; terminal alkenyl groups are grafted onto the stearic acid-modified triacetyl cellulose to obtain a terminal alkenyl triacetyl cellulose derivative; and finally, the terminal alkenyl triacetyl cellulose undergoes olefin polymerization to obtain the highly flexible optical film material for polarizers.
[0007] The method for preparing the highly flexible optical film material for polarizer comprises the following steps:
[0008] 1) Place cellulose in dimethylacetamide and activate it for 10-15 hours, then add the activated cellulose to lithium chloride-dimethylacetamide solution and stir to dissolve for 1-2 hours, add acetic anhydride, stearic acid and concentrated sulfuric acid, react for 0.5-1 hour, add the obtained reaction solution into water, filter, wash the obtained filter cake 2-3 times, and dry to obtain stearic acid-modified cellulose triacetate;
[0009] 2) Stearic acid-modified cellulose triacetate, propylene bromide and sodium hydride are added to tetrahydrofuran, stirred and mixed evenly, and then heated to 50-60°C for reaction for 10-12 hours. After the reaction is completed, water is added to quench the reaction, and then dichloromethane is added to separate the organic layer, and the solvent is removed by vacuum distillation to obtain a terminal cellulose triacetate derivative;
[0010] 3) Add terminal cellulose triacetate derivative and azobisisobutyronitrile to dimethyl sulfoxide, heat to 70-90°C for reaction for 12-24 hours, and after the reaction, remove the solvent by vacuum distillation. Wash the residue with acetone for 3-5 times and dry it to obtain a highly flexible optical film material for polarizers.
[0011] The mass concentration of the lithium chloride-dimethylacetamide solution in step 1) is 8-10%.
[0012] The mass ratio of cellulose, dimethylacetamide, lithium chloride-dimethylacetamide, acetic anhydride, stearic acid, concentrated sulfuric acid and water in step 1) is 1:5-10:10-15:2-2.5:0.9-1.2:0.12-0.25:20-30.
[0013] The mass ratio of the stearic acid-modified cellulose triacetate, propylene bromide, sodium hydride, tetrahydrofuran, water and dichloromethane in step 2) is 1:0.2~1:0.05~0.2:5~10:5~8:10~15.
[0014] The mass ratio of the terminal alkenyl triacetate cellulose derivative, azobisisobutyronitrile and dimethyl sulfoxide in step 3) is 1-1.5:0.001-0.01:10-20.
[0015] Compared with the prior art, the present invention has the following advantages:
[0016] The high-flexibility optical film material for polarizers of the present invention is prepared by modifying cellulose with stearic acid and introducing a small amount of long-chain stearate into triacetyl cellulose, thereby increasing the distance between molecular chains, improving the activity of the molecular chains, and improving the flexibility of the material.
[0017] The high-flexibility optical film material for polarizers of the present invention is prepared by grafting terminal olefin groups onto triacetyl cellulose modified with stearic acid, and wrapping polyethylene on the surface of the triacetyl cellulose through polymerization of vinyl groups, thereby improving the tensile strength, cracking strength, wear resistance and flexibility of the material. In addition, the polyethylene is easy to form a film, and the film is transparent after forming, and will not affect the optical properties of the triacetyl cellulose.
[0018] The high-flexibility optical film material for polarizer prepared by the present invention has excellent optical properties, strong flexibility, good mechanical properties and broad application prospects. DETAILED DESCRIPTION
[0019] In order to better understand the technical solution of the present invention, the above content of the present invention is further described in detail below through specific implementation methods in the form of embodiments, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples. All technologies realized based on the above content of the present invention belong to the scope of the present invention.
[0020] Example 1 0.1 kg of cellulose was placed in 0.5 kg of dimethylacetamide and activated for 10 hours. The activated cellulose was then added to 1 kg of 10% lithium chloride-dimethylacetamide solution and stirred for dissolution for 1 hour. 0.2 kg of acetic anhydride, 0.09 kg of stearic acid and 0.012 kg of concentrated sulfuric acid were added thereto and reacted for 0.5 hours. The obtained reaction solution was added to 2 kg of water and filtered. The obtained filter cake was washed twice and dried to obtain stearic acid-modified cellulose triacetate.
[0021] 0.1 kg of stearic acid-modified cellulose triacetate, 0.02 kg of propylene bromide and 0.005 kg of sodium hydride were added to 0.5 kg of tetrahydrofuran, stirred and mixed evenly, and then heated to 50°C for reaction for 12 hours. After the reaction was completed, 0.5 kg of water was added to quench the reaction, and then 1 kg of dichloromethane was added, the organic layer was separated, and the solvent was removed by reduced pressure distillation to obtain a terminal cellulose triacetate derivative;
[0022] 0.1 kg of terminal cellulose triacetate derivative and 0.1 g of azobisisobutyronitrile were added to 1 kg of dimethyl sulfoxide, heated to 70°C for reaction for 24 hours. After the reaction was completed, the solvent was removed by vacuum distillation, and the residue was washed three times with acetone and dried to obtain a highly flexible optical film material for polarizers.
[0023] Example 2 0.1 kg of cellulose was placed in 0.6 kg of dimethylacetamide and activated for 11 hours. The activated cellulose was then added to 1.1 kg of lithium chloride-dimethylacetamide solution with a mass concentration of 9%, and stirred for dissolution for 1.2 hours. 0.21 kg of acetic anhydride, 0.1 kg of stearic acid and 0.015 kg of concentrated sulfuric acid were added thereto and reacted for 0.6 hours. The obtained reaction solution was added to 2.2 kg of water and filtered. The obtained filter cake was washed twice and dried to obtain stearic acid-modified cellulose triacetate.
[0024] 0.1 kg of stearic acid-modified cellulose triacetate, 0.04 kg of propylene bromide and 0.008 kg of sodium hydride were added to 0.6 kg of tetrahydrofuran, stirred and mixed evenly, and then heated to 52°C for 11 hours. After the reaction was completed, 0.6 kg of water was added to quench the reaction, and then 1.1 kg of dichloromethane was added, the organic layer was separated, and the solvent was removed by reduced pressure distillation to obtain a terminal cellulose triacetate derivative;
[0025] 0.11 kg of terminal cellulose triacetate derivative and 0.3 g of azobisisobutyronitrile were added to 1.2 kg of dimethyl sulfoxide, heated to 75°C for reaction for 20 hours. After the reaction was completed, the solvent was removed by vacuum distillation, and the residue was washed three times with acetone and dried to obtain a highly flexible optical film material for polarizers.
[0026] Example 3 0.1 kg of cellulose was placed in 0.75 kg of dimethylacetamide, activated for 12 hours, and then the activated cellulose was added to 1.2 kg of lithium chloride-dimethylacetamide solution with a mass concentration of 9%, stirred and dissolved for 1.5 hours, 0.22 kg of acetic anhydride, 0.11 kg of stearic acid and 0.018 kg of concentrated sulfuric acid were added thereto, reacted for 0.7 hours, and the obtained reaction solution was added to 2.5 kg of water, filtered, and the obtained filter cake was washed 3 times and dried to obtain stearic acid-modified cellulose triacetate;
[0027] 0.1 kg of stearic acid-modified cellulose triacetate, 0.05 kg of propylene bromide and 0.01 kg of sodium hydride were added to 0.7 kg of tetrahydrofuran, stirred and mixed evenly, and then heated to 55°C for 11 hours. After the reaction was completed, 0.7 kg of water was added to quench the reaction, and then 1.2 kg of dichloromethane was added, the organic layer was separated, and the solvent was removed by vacuum distillation to obtain a terminal cellulose triacetate derivative;
[0028] 0.12 kg of terminal cellulose triacetate derivative and 0.5 g of azobisisobutyronitrile were added to 1.5 kg of dimethyl sulfoxide, heated to 80°C for reaction for 18 hours. After the reaction was completed, the solvent was removed by vacuum distillation, and the residue was washed three times with acetone and dried to obtain a highly flexible optical film material for polarizers.
[0029] Example 4 0.1 kg of cellulose was placed in 0.8 kg of dimethylacetamide and activated for 13 hours. The activated cellulose was then added to 1.3 kg of 10% lithium chloride-dimethylacetamide solution and stirred for dissolution for 1.7 hours. 0.23 kg of acetic anhydride, 0.11 kg of stearic acid and 0.02 kg of concentrated sulfuric acid were added thereto and reacted for 0.85 hours. The obtained reaction solution was added to 2.7 kg of water and filtered. The obtained filter cake was washed 3 times and dried to obtain stearic acid-modified cellulose triacetate.
[0030] 0.1 kg of stearic acid-modified cellulose triacetate, 0.07 kg of propylene bromide and 0.015 kg of sodium hydride were added to 0.9 kg of tetrahydrofuran, stirred and mixed evenly, and then heated to 58°C for 11 hours. After the reaction was completed, 0.75 kg of water was added to quench the reaction, and then 1.4 kg of dichloromethane was added, the organic layer was separated, and the solvent was removed by vacuum distillation to obtain a terminal cellulose triacetate derivative;
[0031] 0.14 kg of terminal cellulose triacetate derivative and 0.6 g of azobisisobutyronitrile were added to 1.7 kg of dimethyl sulfoxide, heated to 85°C for reaction for 15 hours. After the reaction was completed, the solvent was removed by vacuum distillation, and the residue was washed 4 times with acetone and dried to obtain a highly flexible optical film material for polarizers.
[0032] Example 5 0.1 kg of cellulose was placed in 1 kg of dimethylacetamide and activated for 15 hours. The activated cellulose was then added to 1.5 kg of 8% lithium chloride-dimethylacetamide solution and stirred for dissolution for 2 hours. 0.25 kg of acetic anhydride, 0.12 kg of stearic acid and 0.025 kg of concentrated sulfuric acid were added thereto and reacted for 1 hour. The obtained reaction solution was added to 3 kg of water and filtered. The obtained filter cake was washed 3 times and dried to obtain stearic acid-modified cellulose triacetate.
[0033] 0.1 kg of stearic acid-modified cellulose triacetate, 0.1 kg of propylene bromide and 0.02 kg of sodium hydride were added to 1 kg of tetrahydrofuran, stirred and mixed evenly, and then heated to 60°C for reaction for 10 hours. After the reaction was completed, 0.8 kg of water was added to quench the reaction, and then 1.5 kg of dichloromethane was added, the organic layer was separated, and the solvent was removed by reduced pressure distillation to obtain a terminal cellulose triacetate derivative;
[0034] 0.15 kg of terminal cellulose triacetate derivative and 1 g of azobisisobutyronitrile were added to 2 kg of dimethyl sulfoxide, heated to 90°C for reaction for 12 hours. After the reaction was completed, the solvent was removed by vacuum distillation. The residue was washed with acetone 5 times and dried to obtain a highly flexible optical film material for polarizers.
[0035] Example 6 0.1 kg of cellulose was placed in 1 kg of dimethylacetamide and activated for 10 hours. The activated cellulose was then added to 1.5 kg of 10% lithium chloride-dimethylacetamide solution and stirred for dissolution for 1 hour. 0.25 kg of acetic anhydride, 0.09 kg of stearic acid and 0.02 kg of concentrated sulfuric acid were added thereto and reacted for 0.5 hours. The obtained reaction solution was added to 2.5 kg of water and filtered. The obtained filter cake was washed 3 times and dried to obtain stearic acid-modified cellulose triacetate.
[0036] 0.1 kg of stearic acid-modified cellulose triacetate, 0.02 kg of propylene bromide and 0.01 kg of sodium hydride were added to 1 kg of tetrahydrofuran, stirred and mixed evenly, and then heated to 60°C for reaction for 12 hours. After the reaction was completed, 0.8 kg of water was added to quench the reaction, and then 1.5 kg of dichloromethane was added, the organic layer was separated, and the solvent was removed by vacuum distillation to obtain a terminal cellulose triacetate derivative;
[0037] 0.15 kg of terminal cellulose triacetate derivative and 0.1 g of azobisisobutyronitrile were added to 1.5 kg of dimethyl sulfoxide, heated to 90°C for reaction for 12 hours. After the reaction was completed, the solvent was removed by vacuum distillation, and the residue was washed 4 times with acetone and dried to obtain a highly flexible optical film material for polarizers.
[0038] The highly flexible optical film materials for polarizers prepared in Examples 1 to 6 were tested according to the method in GB / T 37384-2019, wherein the polymerization degree test method is as follows: 1 g of the highly flexible optical film material for polarizers was added to 200 mL of a mixed solvent of dichloromethane and ethanol in a volume ratio of 9:1 to obtain a sample solution, and then the outflow time of the sample solution and the mixed solvent was measured by a viscometer, respectively, to calculate the polymerization degree, and the calculation formula of the polymerization degree was:
[0039]
[0040] Wherein DP is the degree of polymerization, 141 is the empirical constant, t1 is the time for the sample solution to flow out, and t2 is the time for the mixed solvent to flow out. The test results are shown in Table 1.
[0041] Table 1 Performance parameter results of materials prepared in Examples 1 to 6
[0042]
[0043] It can be seen from the results in Table 1 that the high-flexibility optical film material for polarizer prepared by the present invention has a high degree of polymerization and a combined acid content of more than 61%.
[0044] 0.1 kg of the highly flexible optical film material for polarizer prepared in Examples 1 to 6 was added to 0.6 kg of a mixed solvent of dichloromethane and ethanol, wherein the mass ratio of dichloromethane to ethanol was 9:1; the mixture was stirred for 10 hours, and the obtained casting solution was poured onto a clean glass plate of an automatic coating machine, and the coating thickness was 200 μm. After coating, the film was allowed to stand, and then dried at 60°C to obtain a TCA optical film. The obtained TCA optical film was tested. The test results are shown in Table 2.
[0045] Table 2 Test results of optical film properties prepared from materials of Examples 1 to 6
[0046]
[0047] It can be seen from the results in Table 2 that the TCA optical film prepared using the high-flexibility optical film material for polarizers of the present invention has high strength and toughness, good mechanical properties, and also has excellent optical properties, high light transmittance and low haze, and has good application prospects in the field of flexible optical materials.
[0048] Although the above describes the specific implementation methods of the present invention, it does not limit the scope of protection of the present invention. Based on the technical solution of the present invention, various modifications or variations that can be made by those skilled in the art without creative work are still within the scope of protection of the present invention.
Claims
1. A highly flexible optical film material for polarizers, characterized by: The method is as follows: cellulose is modified with stearic acid to obtain stearic acid-modified cellulose triacetate; terminal alkenyl groups are grafted onto the stearic acid-modified cellulose triacetate to obtain a terminal alkenyl cellulose triacetate derivative; and finally, the terminal alkenyl cellulose triacetate is polymerized to obtain a highly flexible optical film material for polarizers. The following steps are involved: 1) Cellulose is activated in dimethylacetamide for 10-15 hours, then the activated cellulose is added to a lithium chloride-dimethylacetamide solution and stirred to dissolve for 1-2 hours. Acetic anhydride, stearic acid, and concentrated sulfuric acid are added thereto and reacted for 0.5-1 hour. The resulting reaction solution is added to water and filtered. The resulting filter cake is washed 2-3 times and dried to obtain stearic acid-modified cellulose triacetate. 2) Stearic acid-modified cellulose triacetate, propylene bromide, and sodium hydride are added to tetrahydrofuran, stirred and mixed, and then heated to 50-60°C for 10-12 hours. After the reaction is complete, water is added to quench the reaction, and dichloromethane is added. The organic layer is separated and the solvent is removed by vacuum distillation to obtain a terminal alkenyl cellulose triacetate derivative. 3) Adding a terminal olefin triacetate cellulose derivative and azobisisobutyronitrile to dimethyl sulfoxide, heating to 70-90°C for 12-24 hours, and then removing the solvent by vacuum distillation. The resulting residue is washed with acetone 3-5 times and dried to obtain a highly flexible optical film material for polarizers.
2. The method for preparing the highly flexible optical film material for polarizer according to claim 1, characterized in that: The following steps are involved: 1) Cellulose is activated in dimethylacetamide for 10-15 hours, then the activated cellulose is added to a lithium chloride-dimethylacetamide solution and stirred to dissolve for 1-2 hours. Acetic anhydride, stearic acid, and concentrated sulfuric acid are added thereto and reacted for 0.5-1 hour. The resulting reaction solution is added to water and filtered. The resulting filter cake is washed 2-3 times and dried to obtain stearic acid-modified cellulose triacetate. 2) Stearic acid-modified cellulose triacetate, propylene bromide, and sodium hydride are added to tetrahydrofuran, stirred and mixed, and then heated to 50-60°C for 10-12 hours. After the reaction is complete, water is added to quench the reaction, and dichloromethane is added. The organic layer is separated and the solvent is removed by vacuum distillation to obtain a terminal alkenyl cellulose triacetate derivative. 3) Adding a terminal olefin triacetate cellulose derivative and azobisisobutyronitrile to dimethyl sulfoxide, heating to 70-90°C for 12-24 hours, and then removing the solvent by vacuum distillation. The resulting residue is washed with acetone 3-5 times and dried to obtain a highly flexible optical film material for polarizers.
3. The method for preparing a highly flexible optical film material for a polarizer according to claim 2, wherein: The mass concentration of the lithium chloride-dimethylacetamide solution in step 1) is 8-10%.
4. The method for preparing a highly flexible optical film material for a polarizer according to claim 2, wherein: The mass ratio of cellulose, dimethylacetamide, lithium chloride-dimethylacetamide, acetic anhydride, stearic acid, concentrated sulfuric acid and water in step 1) is 1:5-10:10-15:2-2.5:0.9-1.2:0.12-0.25:20-30.
5. The method for preparing a highly flexible optical film material for a polarizer according to claim 2, wherein: The mass ratio of the stearic acid-modified cellulose triacetate, propylene bromide, sodium hydride, tetrahydrofuran, water and dichloromethane in step 2) is 1:0.2~1:0.05~0.2:5~10:5~8:10~15.
6. The method for preparing a highly flexible optical film material for a polarizer according to claim 2, wherein: The mass ratio of the terminal alkenyl triacetate cellulose derivative, azobisisobutyronitrile and dimethyl sulfoxide in step 3) is 1-1.5:0.001-0.01:10-20.
Citation Information
Patent Citations
Protective film for polarizing plate
JP1997113728A
Cellulose composition, cellulose film, modifier for cellulose film, polarizing plate-protecting film, liquid crystal display device and silver halide photographic photosensitive material
JP2005247961A