A prediction method for crack arrest toughness of high-strength thick plates based on property gradient

By analyzing the correlation between crack arrest toughness and performance gradient, core yield strength, side drop weight non-plastic transition temperature and plate thickness of high-strength thick plates, a performance gradient correlation model was established to solve the problem that small-size samples cannot reflect The problem of overall crack arrest performance of high-strength thick plates enables high-precision prediction of crack arrest toughness.

CN118571386BActive Publication Date: 2024-10-25CHINA SHIPBUILDING INDUSTRY CORPORATION NO725 RESEARCH INSTITUTE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411047088.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-01
Publication Date
2024-10-25
Estimated Expiration
2044-08-01

AI Technical Summary

Technical Problem

The sampling position of the small-size alternative test method in the existing technology is relatively single and cannot fully reflect the overall crack arrest performance of the high-strength thick plate, especially when the composition and structure are uneven.

Method used

By analyzing the correlation between crack arrest toughness and performance gradient, core yield strength, side drop weight non-plastic transition temperature and plate thickness of test steel plates of high strength thick plates, the correlation of crack arrest toughness of high strength thick plates based on performance gradients was established Model, using parameters such as Kca (-10℃), T0, TNDT, CVRP0.2, RP0.2 and t for prediction.

Benefits of technology

A correlation model with clear physical mechanism, simple construction, and quick use is established, which can predict the crack arrest toughness of high-strength thick plates with high accuracy, avoids the shortcomings of a single sampling position for small-size samples, and is suitable for yield strengths of 401~537MPa. , high-strength thick plates with a thickness of 60~90mm.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118571386B_ABST
    Figure CN118571386B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of material fracture failure. The present invention provides a prediction method for crack arrest toughness of a high-strength thick plate based on performance gradient, comprising the following steps: performing correlation analysis on crack arrest toughness of a test steel plate of a high-strength thick plate and performance gradient, core yield strength, side drop hammer non-plastic transition temperature and plate thickness; establishing a correlation model for crack arrest toughness of a high-strength thick plate based on performance gradient; when predicting crack arrest toughness of a high-strength thick plate, K is obtained by performing crack arrest test, side drop hammer test and tensile test of the high-strength thick plate. ca(‑10℃) , T0, T NDT 、CV RP0.2 , R P0.2 , K ca(‑10℃) , T0, T NDT 、CV RP0.2 , R P0.2 , t are substituted into formula (1) to determine the parameters α, β, γ. The prediction method of the crack arrest toughness of the high-strength thick plate based on the performance gradient of the present invention can fully reflect the overall crack arrest toughness of the high-strength thick plate.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of material fracture failure research, and in particular to a method for predicting crack arrest toughness of a high-strength thick plate based on performance gradient. Background Art

[0002] With the large-scale and ultra-large-scale container ship structures, in order to meet the stiffness and strength requirements, the strength grade and thickness specifications of the steel plates used in the hull structure are also increasing. The highest strength level has reached 460MPa, and the maximum plate thickness specification is approaching 100mm. With the increase of strength and the increase of plate thickness, the fracture resistance of the steel plate decreases, and the safety and reliability issues are prominent. In order to ensure the safety of the structure, the high-strength thick steel plates used in key parts of large container ships must have crack arresting properties, that is, once brittle cracks occur in the structure, the steel plates can stop them, thereby avoiding catastrophic damage. To this end, the IACS Hull Committee has specially established the PT52 working group to formulate relevant standards for the safe application of 50~100mm thick high-strength steel thick plates for ships, and proposed a crack arresting performance evaluation test method and technical indicators of crack arresting performance (plate thickness ≤80mm, K at -10℃ ca ≥6000N / mm 3 / 2 ; Plate thickness>80mm, K at -10℃ ca ≥8000N / mm 3 / 2 ).

[0003] A large number of studies have been carried out at home and abroad on how to evaluate and regulate crack arrest performance, and a variety of correlation models between crack arrest toughness / crack arrest temperature and small-size specimen characterization parameters have been established. At present, the correlation model between crack arrest toughness and the side non-plastic transition temperature, the correlation model between crack arrest temperature and the core dynamic tear ductile-brittle transition temperature, etc. have been established in China. Among them, the correlation model between crack arrest temperature and the side non-plastic transition temperature has been incorporated into the international specification URW31, and has become one of the three internationally recognized small-size alternative test methods for crack arrest performance. In the prior art, the patent with application number CN202210208937.2 discloses a prediction model for the crack arrest temperature of a thick plate of high-strength steel for ships, its construction method and application. The patent provides a crack arrest temperature prediction model based on a small-size tensile test and a drop hammer test. Foreign countries have successively proposed two small-size alternative test methods for crack arrest performance, including the correlation model between crack arrest temperature and the surface non-plastic transition temperature and the 1 / 4 plate thickness impact ductile-brittle transition temperature, and the correlation model between crack arrest temperature and the temperature corresponding to the specific absorption energy of the pressed notch impact specimen.

[0004] In summary, the prior art seeks a method for a small-size alternative test. The sampling position of the small-size test is relatively single. For high-strength thick plates, the uneven composition and organization lead to an inevitable performance gradient along the thickness direction of the plate. The sample at a single position cannot fully reflect the overall crack arrest performance of the high-strength thick plate.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The purpose of the present invention is to propose a prediction method for the crack arrest toughness of high-strength thick plates based on performance gradient, so as to solve the problem of finding a small-size alternative test method in the prior art. The sampling position of the small-size test is relatively single, and for high-strength thick plates, due to the uneven composition and organization, there is inevitably a performance gradient along the thickness direction of the plate. The sample at a single position cannot fully reflect the overall crack arrest performance of the high-strength thick plate.

[0007] To achieve the above object, the technical solution of the present invention is achieved as follows:

[0008] A method for predicting crack arrest toughness of high-strength thick plates based on performance gradient comprises the following steps:

[0009] S1. Conduct correlation analysis on crack arrest toughness and performance gradient, core yield strength, side drop hammer non-plastic transition temperature and plate thickness of high-strength thick plate test steel plate;

[0010] S2. Establish a crack arrest toughness correlation model of high-strength thick plates based on performance gradient as shown in formula (1);

[0011] ;

[0012] In the formula, K ca(-10℃) ——K at -10℃ ca , N / mm 3 / 2 ; R P0.2 ——Core yield strength, MPa; CV RP0.2 ——Yield strength variation coefficient, MPa; T NDT ——No plastic transition temperature of side drop weight, ℃; T 0 ——Crack arrest toughness K ca -Crack arrest temperature T k Transformation characteristic parameters, ; t——steel plate thickness, mm; α, β, γ——parameters to be determined;

[0013] S3. When predicting the crack arrest toughness of high-strength thick plates, the K is obtained by conducting crack arrest tests, side drop hammer tests and tensile tests on high-strength thick plates. ca(-10℃) 、T 0 、T NDT 、CV RP0.2 , R P0.2 , K ca(-10℃) 、T 0 、T NDT 、CV RP0.2 , R P0.2Substitute , t into formula (1) to determine the parameters α, β, and γ.

[0014] The method for predicting the crack arrest toughness of high-strength thick plates based on performance gradient described in the present invention not only takes into account the performance gradient of the steel plate of the high-strength thick plate, but also takes into account the core yield strength, the side drop hammer non-plastic transition temperature and the plate thickness of the steel plate of the high-strength thick plate, and establishes the coefficient of variation CV of crack arrest toughness and yield strength. RP0.2 , Core yield strength R P0.2 , Crack arrest toughness K ca -Crack arrest temperature T k Transformation characteristic parameter T 0 , Side drop hammer non-plastic transition temperature T NDT , and plate thickness t avoids the problem that a single sampling position of a small-size specimen cannot fully reflect the overall crack arrest performance of a high-strength thick plate. The correlation model has the advantages of clear physical mechanism, simple construction, and quick use.

[0015] Further, in step S1, the crack arrest toughness and performance gradient correlation analysis of the high-strength thick plate test steel plate is carried out, specifically, the crack arrest toughness K of the high-strength thick plate at -10°C is ca The standard deviation SD of the yield strength at the surface, 1 / 4 thickness and center of the test steel plate Rp0.2 , yield strength variation coefficient CV Rp0.2 , tensile strength standard deviation SD Rm and coefficient of variation of tensile strength CV Rm Correlation analysis.

[0016] Further, in step S3, by setting t to 50-90 mm, R P0.2 400~597MPa, T NDT -80~-15℃, CV RP0.2 0.015~0.116, T 0 500~2500 and K ca(-10℃) 2000~13500N / mm 3 / 2 Substituting into the correlation model of formula (1), the least squares method was used for fitting, and the parameters α=4.03, β=0.175, and γ=2.617×10 -10 , we get the prediction model, which is shown in formula (2):

[0017] .

[0018] Furthermore, after determining the parameters of α, β, and γ, there is no need to conduct crack arrest tests when predicting the crack arrest toughness of high-strength thick plates. Only tensile tests and side drop hammer tests are needed to predict the T 0 , TNDT 、CV RP0.2 , R P0.2 Substituting t and t into the prediction model of formula (2) can predict the crack arrest toughness of high-strength thick plates.

[0019] Furthermore, the prediction method is applicable to high-strength thick plates with a yield strength of 401-537 MPa and a thickness of 60-90 mm.

[0020] Compared with the prior art, the prediction method of crack arrest toughness of high-strength thick plates based on performance gradient described in the present invention has the following beneficial effects:

[0021] The method for predicting crack arrest toughness of high-strength thick plates based on performance gradient described in the present invention not only takes into account the performance gradient of the steel plate of the high-strength thick plate, but also takes into account the core yield strength, side drop hammer non-plastic transition temperature and plate thickness of the steel plate of the high-strength thick plate, and establishes the coefficient of variation CV of crack arrest toughness and yield strength. RP0.2 , Core yield strength R P0.2 , Crack arrest toughness K ca -Crack arrest temperature T k Transformation characteristic parameter T 0 , Side drop hammer non-plastic transition temperature T NDT , and plate thickness t, avoids the problem that a single sampling position of a small-size specimen cannot fully reflect the overall crack arrest performance of a high-strength thick plate, and has high prediction accuracy. The correlation model has the advantages of clear physical mechanism, simple construction, and quick use. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a schematic diagram of the change in yield strength of the test steel plate along the plate thickness direction;

[0023] Figure 2 This is a schematic diagram of the change of the ductile-brittle transition temperature of the test steel plate along the plate thickness direction;

[0024] Figure 3 The crack arrest toughness K at -10℃ ca(-10℃) The standard deviation SD of the yield strength at the surface, 1 / 4 thickness and center of the test steel plate Rp0.2 Schematic diagram of the statistical distribution of ;

[0025] Figure 4 The crack arrest toughness K at -10℃ ca(-10℃) The yield strength variation coefficient CV of the test steel plate surface, 1 / 4 plate thickness and center Rp0.2 Schematic diagram of the statistical distribution of ;

[0026] Figure 5 The crack arrest toughness K at -10℃ ca(-10℃)The standard deviation of tensile strength at the surface, 1 / 4 thickness and core of the test steel plate is SD Rm Schematic diagram of the statistical distribution of ;

[0027] Figure 6 The crack arrest toughness K at -10℃ ca(-10℃) Coefficient of variation CV of tensile strength at three locations: surface, 1 / 4 thickness and core of the test steel plate Rm Schematic diagram of the statistical distribution of ;

[0028] Figure 7 K is the crack arrest toughness of the test steel plate ca(-10℃) Schematic diagram of the correlation with the core yield strength;

[0029] Figure 8 K is the crack arrest toughness of the test steel plate ca(-10℃) Schematic diagram of the correlation with the non-plastic transition temperature of the side drop hammer;

[0030] Fig. 9 K is the crack arrest toughness of the test steel plate ca(-10℃) Schematic diagram of the correlation with plate thickness;

[0031] Fig.10 For K ca(-10℃) / R p0.2 / T 0 2 / t 2 and ln(CV Rp0.2 ) / T 0 2 / t 2 Schematic diagram of crack arrest toughness correlation analysis with linear fitting considering temperature and plate thickness effects;

[0032] Fig.11 For K ca(-10℃) / R p0.2 / T 0 2 / t 2 With T NDT / T 0 2 / t 2 Schematic diagram of the crack arrest toughness correlation analysis with linear fitting considering the temperature and plate thickness effects. DETAILED DESCRIPTION

[0033] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The descriptions of "first", "second", etc. mentioned in the embodiments of the present invention are only for descriptive purposes, and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.

[0034] The present invention will be described in detail below with reference to the accompanying drawings and in conjunction with embodiments.

[0035] In the present application, it should be noted that the high-strength thick plate is a steel plate.

[0036] In the prior art, a method of finding a small-size alternative test is used. The sampling position of the small-size test is relatively single. For high-strength thick plates, due to the uneven composition and organization, a performance gradient is inevitably present along the thickness direction of the plate. The sample at a single position cannot fully reflect the overall crack arrest performance of the high-strength thick plate.

[0037] However, there is no public report on the research on the correlation analysis and prediction model of crack arrest toughness of high-strength thick plates with material property gradient and non-plastic transition temperature.

[0038] Based on this, the present invention proposes a prediction method for the crack arrest toughness of high-strength thick plates based on performance gradient. The model can be established through the material's yield strength performance gradient characterization parameters and the non-plastic transition temperature, which can provide guidance for improving the crack arrest performance of high-strength thick plates.

[0039] The purpose of this invention is to propose a prediction model for the crack arrest toughness of high-strength thick plates based on performance gradient, to achieve predictive evaluation of the crack arrest toughness of high-strength thick plates through material property gradient and side drop hammer non-plastic transition temperature measurement, and to provide a basis for improving the crack arrest performance of high-strength thick plates.

[0040] like Figures 1 to 11 As shown, the present invention proposes a prediction method for the crack arrest toughness of a high-strength thick plate based on a performance gradient, the prediction method is applicable to a high-strength thick steel plate with a yield strength of 401-537 MPa and a thickness of 60-90 mm, and the prediction method comprises the following steps:

[0041] S1. Conduct correlation analysis on crack arrest toughness and performance gradient, core yield strength, side drop hammer non-plastic transition temperature and plate thickness of high-strength thick plate test steel plate;

[0042] S2. Establish a crack arrest toughness correlation model of high-strength thick plates based on performance gradient as shown in formula (1);

[0043] ;

[0044] In the formula, K ca(-10℃) ——K at -10℃ ca , N / mm 3 / 2 ; R P0.2 ——Core yield strength, MPa; CV RP0.2 ——Yield strength variation coefficient, MPa; T NDT ——No plastic transition temperature of side drop weight, ℃; T 0 ——Crack arrest toughness K ca -Crack arrest temperature T k Transformation characteristic parameters, ; t——steel plate thickness, mm; α, β, γ——parameters to be determined;

[0045] S3. When predicting the crack arrest toughness of high-strength thick plates, the K is obtained by conducting crack arrest tests, side drop hammer tests and tensile tests on high-strength thick plates. ca(-10℃) , T 0 , T NDT 、CV RP0.2 , R P0.2 , K ca(-10℃) , T 0 , T NDT 、CV RP0.2 , R P0.2 Substitute , t into formula (1) to determine the parameters α, β, and γ.

[0046] The present invention starts from the correlation between the crack arrest toughness and material property gradient of high-strength thick plate and the non-plastic transition temperature of the side drop hammer, and establishes the coefficient of variation C of crack arrest toughness and yield strength by analyzing the correlation between crack arrest toughness and the property gradient along the plate thickness direction and the non-plastic transition temperature of the side drop hammer. VRP0.2 , non-plastic transition temperature and the correlation model, which has the advantages of clear physical mechanism, simple construction and quick use.

[0047] Example 1

[0048] The present invention proposes a method for predicting crack arrest toughness of a high-strength thick plate based on performance gradient, comprising the following steps:

[0049] S1. Conduct correlation analysis on crack arrest toughness and performance gradient, core yield strength, side drop hammer non-plastic transition temperature and plate thickness of high-strength thick plate test steel plate;

[0050] Figure 1To test the change of yield strength ductile-brittle transition temperature of steel plate along the thickness direction, Figure 2 To test the change of ductile-brittle transition temperature of steel plate along the thickness direction, such as Figure 1 and Figure 2 As shown, it can be seen that the yield strength of the high-strength thick plate tends to gradually decrease from the surface to the core, and the ductile-brittle transition temperature of the high-strength thick plate tends to gradually increase from the surface to the core, that is, for the high-strength thick plate, its yield strength and ductile-brittle transition temperature are both distributed in a gradient to a certain extent. Based on the above analysis, the present invention establishes a prediction model for crack arrest toughness through correlation analysis of crack arrest toughness and performance gradient characterization parameters of high-strength thick plates and lateral drop hammer non-plastic transition temperature.

[0051] First, the applicant conducted a correlation analysis between the crack arrest toughness and performance gradient of high-strength thick plates.

[0052] In step S1, the crack arrest toughness and performance gradient correlation analysis of the high-strength thick plate test steel plate is carried out, specifically, the crack arrest toughness K of the high-strength thick plate at -10℃ is ca The standard deviation SD of the yield strength at the surface, 1 / 4 thickness and center of the test steel plate Rp0.2 , yield strength variation coefficient CV Rp0.2 , tensile strength standard deviation SD Rm and coefficient of variation of tensile strength CV Rm Correlation analysis.

[0053] More specifically, the applicant has conducted a study on the crack arrest toughness K of multiple groups of test steel plates at -10°C. ca The yield strength and tensile strength of the test steel plate were tested at the surface, 1 / 4 plate thickness and core, and then the standard deviation SD of the yield strength of multiple groups of test steel plates was calculated. Rp0.2 , yield strength variation coefficient CV Rp0.2 , tensile strength standard deviation SD Rm and coefficient of variation of tensile strength CV Rm Conduct statistical analysis, such as Figure 3 , Figure 4 , Figure 5 and Figure 6 shown.

[0054] The test data are for 390MPa and 460MPa grade crack arrest thick plates, with plate thickness ranging from 50 to 90mm and yield strength standard deviation SD Rp0.2 , yield strength variation coefficient CV Rp0.2 , tensile strength standard deviation SD Rm and coefficient of variation of tensile strength CV Rm It is calculated based on data measured at three locations: the surface of high-strength thick plates, 1 / 4 of the plate thickness, and the center.

[0055] like Figures 3 to 6 As shown, overall, with the SD Rp0.2 、CV Rp0.2 , SD Rm and CV Rm The increase of crack arrest toughness K ca(-10℃) In comparison, Figure 6 As shown, the crack arrest toughness K ca(-10℃) Coefficient of variation of tensile strength CV Rm Relationships are more discrete, such as Figure 4 As shown, the crack arrest toughness K ca(-10℃) Coefficient of variation of yield strength CV Rp0.2 The correlation is quite obvious.

[0056] Based on the above analysis, the applicant believes that the yield strength variation coefficient CV Rp0.2 It is an important factor affecting the crack arrest toughness of materials.

[0057] Secondly, the applicant conducted a correlation analysis on the crack arrest toughness of high-strength thick plates with the core yield strength, the side drop hammer non-plastic transition temperature and the plate thickness, such as Figure 7 , Figure 8 and Fig. 9 shown.

[0058] Figure 7 It is a schematic diagram of the correlation between the crack arrest toughness and the core yield strength of the test steel plate. Figure 7 As shown in the figure, as the core yield strength increases, the crack arrest toughness K ca(-10℃) There is an upward trend, but the data is relatively discrete; Figure 8 The figure is a schematic diagram of the correlation between the crack arrest toughness of the test steel plate and the non-plastic transition temperature of the side drop hammer. Figure 8 As shown in the figure, with the increase of the non-plastic transition temperature of the side drop hammer, the crack arrest toughness K ca(-10℃) There is a clear downward trend, but the data are somewhat discrete; Fig. 9 The schematic diagram of the correlation between the crack arrest toughness of the test steel plate and the plate thickness is as follows: Fig. 9 As shown in the figure, with the increase of plate thickness, K ca(-10℃) Shows a decreasing trend.

[0059] Based on the above analysis, the applicant believes that the core yield strength, the side drop weight non-plastic transition temperature and plate thickness are all important factors affecting the crack arrest toughness of high-strength thick plates, but there is a certain degree of discreteness in the correlation with a single factor.

[0060] S2. Then, the applicant considered the factors affecting the crack arrest toughness of high-strength thick plates by considering the temperature and plate thickness effects. Based on the above analysis, it can be seen that the yield strength performance gradient, the core yield strength, and the side drop hammer non-plastic transition temperature all affect the crack arrest toughness of high-strength thick plates. The influence of plate thickness and temperature was examined, and the plate thickness effect parameter t was introduced.2 and temperature effect parameter T 0 2 Modified yield strength coefficient of variation CV Rp0.2 = ln(CV Rp0.2 ) / T 0 2 / t 2 , corrected side drop hammer non-plastic transition temperature T NDT T NDT / T 0 2 / t 2 , and introduce the core yield strength R p0.2 Correction K ca(-10℃) K ca(-10℃) / R p0.2 / T 0 2 / t 2 .

[0061] The applicant's ca(-10℃) / R p0.2 / T 0 2 / t 2 and ln(CV Rp0.2 ) / T 0 2 / t 2 Perform a linear fit, such as Fig.10 As shown, K ca(-10℃) / R p0.2 / T 0 2 / t 2 and ln(CV Rp0.2 ) / T 0 2 / t 2 There is a linear relationship, as ln(CV Rp0.2 ) / T 0 2 / t 2 The increase of K ca(-10℃) / R p0.2 / T 0 2 / t 2 Showing a downward trend.

[0062] The applicant also requested K ca(-10℃) / R p0.2 / T 0 2 / t 2 With T NDT / T 0 2 / t 2 Perform a linear fit, such as Fig.11 As shown, Kca(-10℃) / R p0.2 / T 0 2 / t 2 With T NDT / T 0 2 / t 2 It is a linear relationship, with T NDT / T 0 2 / t 2 The increase of K ca(-10℃) / R p0.2 / T 0 2 / t 2 Showing a downward trend.

[0063] Based on the above analysis, the applicant believes that K ca(-10℃) / R p0.2 / T 0 2 / t 2 Not only with ln(CV Rp0.2 ) / T 0 2 / t 2 Related to T NDT / T 0 2 / t 2 Related.

[0064] In summary, the crack arrest toughness K ca(-10℃) Coefficient of variation of yield strength CV RP0.2 , Core yield strength R P0.2 , Side drop hammer non-plastic transition temperature T NDT , plate thickness t, crack arrest toughness K ca -Crack arrest temperature T k Transformation characteristic parameter T 0 There is a close relationship between them, that is, the crack arrest toughness of high-strength thick plates mainly depends on CV RP0.2 , R P0.2 , T NDT , T 0 and t.

[0065] Therefore, the applicant established a correlation model of crack arrest toughness of high-strength thick plates based on performance gradient as shown in formula (1);

[0066]

[0067] In the formula, K ca(-10℃) ——K at -10℃ ca , N / mm 3 / 2 ; R P0.2——Core yield strength, MPa; CV RP0.2 ——Yield strength variation coefficient, MPa; T NDT ——No plastic transition temperature of side drop weight, ℃; T 0 ——Crack arrest toughness K ca -Crack arrest temperature T k Transformation characteristic parameters, ; t——steel plate thickness, mm; α, β, γ——parameters to be determined.

[0068] S3. When predicting the crack arrest toughness of high-strength thick plates, the K is obtained by conducting crack arrest tests, side drop hammer tests and tensile tests on high-strength thick plates. ca(-10℃) , T 0 , T NDT 、CV RP0.2 , R P0.2 , K ca(-10℃) , T 0 , T NDT 、CV RP0.2 , R P0.2 Substitute , t into formula (1) to determine the parameters α, β, and γ.

[0069] Specifically, when predicting the crack arrest toughness of high-strength thick plates, the applicant shall follow ISO 20064-2019 "Metallic Materials - Steel - Brittle Crack Arrest Toughness K ca Test method》Carry out crack arrest test on different batches of high-strength thick plates to obtain the crack arrest toughness K at -10℃ ca(-10℃) and T, which characterizes the trend of crack arrest toughness changing with temperature 0 According to GB / T6803 "Drop-hammer test method for non-plastic transition temperature of ferritic steel", the side drop-hammer test was carried out to obtain the non-plastic transition temperature T NDT ; According to GB / T228.1 "Metallic Materials Tensile Test Part 1 Room Temperature Test Method" tensile test was carried out to obtain the surface yield strength, 1 / 4 plate thickness yield strength and core yield strength R of high-strength thick plates P0.2 , calculate the yield strength coefficient of variation CV RP0.2 , the data are shown in Table 1.

[0070] Table 1

[0071]

[0072] By setting t to 50~90mm, R P0.2 400~597MPa, T NDT -80~-15℃, CV RP0.2 0.015~0.116, T 0 500~2500 and K ca(-10℃)2000~13500N / mm 3 / 2 Substituting into the correlation model of formula (1), the least square method was used for fitting. As shown in Table 2, the parameters α=4.03, β=0.175, and γ=2.617×10 -10 , we get the prediction model, which is shown in formula (2):

[0073] .

[0074] Table 2 Undetermined parameter values ​​in the calculation model

[0075]

[0076] After determining the parameters of α, β, and γ, there is no need to conduct crack arrest tests when predicting the crack arrest toughness of high-strength thick plates. Only tensile tests and side drop hammer tests are needed to predict the T 0 , T NDT 、CV RP0.2 , R P0.2 Substituting t and t into the prediction model of formula (2) can predict the crack arrest toughness of high-strength thick plates.

[0077] To this end, the applicant obtained T values ​​for 15 groups of typical steel plates through tensile tests and side drop weight tests. 0 , T NDT 、CV RP0.2 , R P0.2 and t, T 0 , T NDT 、CV RP0.2 , R P0.2 Substituting t and t into equation (2) can predict the crack arrest toughness K of high-strength thick plate. ca(-10℃) The applicant obtained the crack arrest toughness K at -10℃ through crack arrest tests on 15 groups of typical steel plates. ca(-10℃) The applicant compared the measured value of crack arrest toughness with the predicted value, and the results are shown in Table 3.

[0078] Table 3 Comparison of crack arrest toughness prediction and measured values

[0079]

[0080] As shown in Table 3, the crack arrest toughness can be predicted by the prediction method of the present invention with high prediction accuracy and prediction deviations less than 1700 N / mm. 3 / 2 , which can meet the requirements of material research and development and trial production. As shown in Table 3, the prediction method of the present invention is suitable for predicting the crack arrest toughness of high-strength thick plates with a yield strength of 401-537 MPa and a thickness of 60-90 mm.

[0081] Although the present invention is disclosed as above, the present invention is not limited thereto. Any person skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the protection scope of the present invention shall be subject to the scope defined by the claims.

Claims

1. A method for predicting crack arrest toughness of high-strength thick plates based on performance gradient, characterized in that: The following steps are involved: S1. Conduct correlation analysis on crack arrest toughness and performance gradient, core yield strength, side drop hammer non-plastic transition temperature and plate thickness of high-strength thick plate test steel plate; S2. Establish a crack arrest toughness correlation model of high-strength thick plates based on performance gradient as shown in formula (1); , In the formula, K ca(-10℃) ——K at -10℃ ca , N / mm 3 / 2 ; R P0.2 ——Core yield strength, MPa; CV RP0.2 ——yield strength variation coefficient, MPa; T NDT ——No plastic transition temperature of side drop hammer, ℃; T0——Crack arrest toughness K ca -Crack arrest temperature T k Transformation characteristic parameters, ; t——steel plate thickness, mm; α, β, γ——parameters to be determined; S3. When predicting the crack arrest toughness of high-strength thick plates, the K is obtained by conducting crack arrest tests, side drop hammer tests and tensile tests on high-strength thick plates. ca(-10℃) , T0, T NDT 、CV RP0.2 , R P0.2 , K ca(-10℃) , T0, T NDT 、CV RP0.2 , R P0.2 , t are substituted into formula (1) to determine the parameters α, β, γ; In step S3, by setting t to 50-90 mm, R P0.2 400~597MPa, T NDT -80~-15℃, CV RP0.2 0.015~0.116, T0 500~2500 and K ca(-10℃) 2000~13500N / mm 3 / 2 Substituting into the correlation model of formula (1), the least squares method is used for fitting, and the parameters α=4.03, β=0.175, γ=2.617×10-10 are determined to obtain the prediction model, which is shown in formula (2): 。 2. The prediction method of crack arrest toughness of high-strength thick plate based on performance gradient according to claim 1 is characterized in that: In step S1, the crack arrest toughness and performance gradient correlation analysis of the high-strength thick plate test steel plate is carried out, specifically, the crack arrest toughness K of the high-strength thick plate at -10℃ is ca The standard deviation SD of the yield strength at the surface, 1 / 4 thickness and center of the test steel plate Rp0.2 , yield strength variation coefficient CV Rp0.2 , tensile strength standard deviation SD Rm and coefficient of variation of tensile strength CV Rm Correlation analysis.

3. The prediction method of crack arrest toughness of high-strength thick plate based on performance gradient according to claim 1, characterized in that: After determining the parameters of α, β, and γ, there is no need to conduct crack arrest tests when predicting the crack arrest toughness of high-strength thick plates. Only tensile tests and side drop hammer tests are needed to calculate T0 and T2. NDT 、CV RP0.2 , R P0.2 Substituting t and t into the prediction model of formula (2) can predict the crack arrest toughness of high-strength thick plates.

4. The method for predicting crack arrest toughness of high-strength thick plates based on performance gradient according to claim 3, characterized in that: The prediction method is applicable to high-strength thick plates with a yield strength of 401-537 MPa and a thickness of 60-90 mm.