A method for making inner and outer rings of bearings

Through powder metallurgy and warm composite extrusion technology, combined with heat treatment and finishing, the problem of material waste and long production cycle in the traditional bearing inner and outer ring ring blanking method has been solved, and efficient and low-cost bearing inner and outer ring ring parts production has been achieved. , ensuring the dimensional accuracy and performance stability of the product.

CN118577795BActive Publication Date: 2024-10-22XI AN SINOBERUN HEAVY IND TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411076705.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-10-22
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

The traditional method of making the inner and outer rings of bearings has the problems of material waste, long production cycle, high cost and unstable dimensional accuracy.

Method used

Using powder metallurgy technology of high-purity bearing steel powder and additives, the billet is formed through isostatic pressing and warm composite extrusion technology, combined with heat treatment and finishing, to simplify process steps and achieve automated continuous production.

Benefits of technology

Significantly reduce material waste, shorten the production cycle, reduce manufacturing costs, improve product dimensional accuracy and performance stability, and enhance market competitiveness.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

This invention discloses a method for preparing inner and outer ring components of a bearing, relating to the field of bearing manufacturing technology. High-purity bearing steel powder is selected and mixed with additives at a mass ratio of 95:5-98:2. The mixed bearing steel powder is placed in a mold and pressed using isostatic pressing at 250-300 MPa for 60 seconds to form a blank. Employing powder metallurgy and warm composite extrusion technology, the pressing and extrusion processes minimize material waste and improve material utilization. The manufacturing process of the inner and outer ring components of the bearing is simplified by integrating powder pressing, warm composite extrusion, heat treatment, and finishing into a single system, significantly shortening the production cycle. This results in relatively lower manufacturing costs, enhancing market competitiveness. Through simulation analysis and precise control of parameters such as temperature and pressure, the material's flowability and deformation behavior during the forming process are ensured to meet expectations, thereby guaranteeing the dimensional accuracy and performance stability of the product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of bearing manufacturing, and in particular to a method for making inner and outer ring parts of a bearing. Background Art

[0002] The traditional method of making inner and outer rings of bearings often leads to a large waste of materials and reduces the utilization rate of materials due to the limitations of material fluidity and molding process when making inner and outer rings of bearings. It also requires multiple complex process steps, such as heating, forging, cooling, heat treatment, etc. Each step takes a certain amount of time, resulting in a long overall production cycle and relatively high manufacturing costs, which is not conducive to market competition. It is also easily affected by various factors during the molding process, such as temperature, pressure, equipment accuracy, etc., resulting in unstable product dimensional accuracy and performance.

[0003] In view of this, the present invention is proposed. Summary of the invention

[0004] The purpose of this application is to provide a method for manufacturing inner and outer rings of a bearing, comprising the following steps:

[0005] S1. Select high-purity bearing steel powder and mix it with additives in a mass ratio of 95:5-98:2;

[0006] S2, putting the mixed bearing steel powder into a mold, and pressing it at 250-300 MPa for 60 seconds by isostatic pressing technology to form a blank;

[0007] S3. Place the pressed billet into a warm composite extruder, control the extrusion temperature to 1100±5°C, and extrude at a speed of 10±0.1mm / s to cause the billet to undergo plastic deformation to form the required inner and outer ring shapes of the bearing;

[0008] S4. Heat treatment is performed on the extruded inner and outer rings of the bearing to improve the structure and performance of the material;

[0009] S5. Finish the inner and outer rings of the bearing after heat treatment to ensure that their dimensional accuracy and surface quality meet the requirements;

[0010] Among them, heat treatment includes normalizing, quenching and tempering;

[0011] The normalizing temperature is 920℃ and the holding time is 2h;

[0012] The quenching temperature is 840℃ and the holding time is 1h;

[0013] The tempering temperature is 600℃ and the holding time is 2h.

[0014] Furthermore, the accuracy of the mold is ±0.01 mm, and the surface roughness is less than Ra0.8 μm.

[0015] Furthermore, the grinding depth of the finishing process is 0.01 mm and the polishing speed is 2000 rpm.

[0016] Furthermore, additives include lubricants, antioxidants and alloying elements, and the alloying elements include carbon, chromium, manganese, silicon, molybdenum, vanadium and titanium.

[0017] By adopting the above technical solution, the present invention has the following beneficial effects:

[0018] 1. The use of powder metallurgy and warm composite extrusion technology can minimize material waste and improve material utilization by accurately controlling the powder ratio, pressing and extrusion process.

[0019] 2. The blank making method provided in this application simplifies the production process steps of inner and outer rings of bearings, integrates the steps of powder pressing, warm composite extrusion, heat treatment and finishing into one system, and significantly shortens the production cycle through automation and continuous production.

[0020] 3. Due to the shortened material utilization rate and production cycle, the manufacturing cost is relatively reduced, which is conducive to improving market competitiveness.

[0021] 4. Through simulation analysis and precise control of parameters such as temperature and pressure, the fluidity and deformation behavior of the material during the molding process are ensured to meet expectations, thereby ensuring the dimensional accuracy and performance stability of the product. DETAILED DESCRIPTION

[0022] The embodiment of the present application provides a method for manufacturing inner and outer rings of a bearing, comprising the following steps:

[0023] S1. Select high-purity bearing steel powder to ensure that the physical and chemical properties of the material meet the requirements of the inner and outer rings of the bearing, and mix it with the additives in a mass ratio of 95:5-98:2 to ensure the uniformity and stability of the raw materials;

[0024] S2. Put the mixed bearing steel powder into a mold, and press it at 250-300 MPa for 60 seconds by isostatic pressing technology to form a blank. The isostatic pressing technology is divided into cold isostatic pressing technology, warm isostatic pressing technology and hot isostatic pressing technology. The embodiment of the present application uses hot isostatic pressing technology. The pressing temperature is 1000-2200°C. Under the simultaneous action of high temperature and high pressure, the material is subjected to isostatic pressing, thereby ensuring uniform stress distribution inside the blank and avoiding deformation and cracking in subsequent processing;

[0025] S3. Put the pressed billet into a warm composite extruder, control the extrusion temperature to 1100±5℃, and extrude at a speed of 10±0.1mm / s. This extrusion speed ensures the stability of the molding process and the reliability of the finished product quality, so that the billet undergoes plastic deformation to form the required inner and outer ring shapes of the bearing. The warm composite extruder can realize efficient and accurate molding of billets of different materials, shapes and sizes. During the extrusion process of the warm composite extruder, the temperature and extrusion speed should be accurately controlled. The temperature control should ensure that the billet undergoes plastic deformation at an appropriate temperature to avoid degradation of material properties or deformation and cracking due to excessively high or low temperatures. The extrusion speed should be adjusted according to the properties of the material and molding requirements to ensure the stability of the molding process and the reliability of the finished product quality. The size and shape of the extruded inner and outer rings of the bearing are tested, including diameter, wall thickness, ovality, etc., to ensure that the quality of the finished product meets the design requirements.

[0026] S4. Heat treatment is performed on the extruded inner and outer rings of the bearing to improve the structure and performance of the material;

[0027] S5. Finish the inner and outer rings of the bearing after heat treatment to ensure that their dimensional accuracy and surface quality meet the requirements. Grinding should ensure that the dimensional accuracy and surface roughness of the inner and outer rings of the bearing meet the design requirements. Polishing should improve the surface finish and reduce the surface roughness of the inner and outer rings of the bearing. Strict quality inspection should be carried out on the inner and outer rings of the bearing after finishing, including dimensional accuracy, shape accuracy, surface quality, etc., to ensure that the product quality meets the standards.

[0028] In the above scheme, powder metallurgy and warm composite extrusion technology are used to accurately control the powder ratio, pressing and extrusion process, which can minimize material waste and improve material utilization. The blank making method provided in this application simplifies the production process steps of inner and outer rings of bearings, integrates powder pressing, warm composite extrusion, heat treatment and finishing steps into one system, and significantly shortens the production cycle through automation and continuous production. Due to the shortening of material utilization and production cycle, the manufacturing cost is relatively reduced, which is conducive to improving market competitiveness. Through simulation analysis and precise control of parameters such as temperature and pressure, the fluidity and deformation behavior of the material during the molding process are ensured to meet expectations, thereby ensuring the dimensional accuracy and performance stability of the product.

[0029] The precision of the mold is ±0.01mm, and the surface roughness is less than Ra0.8μm to ensure that the shape and size of the pressed billet are accurate. When using isostatic pressing technology for pressing, the isostatic pressing technology ensures uniform stress distribution inside the billet by applying uniform pressure in all directions. The pressure and pressing time should be precisely controlled during the pressing process to ensure that the density and strength of the billet meet the requirements. The size and shape of the pressed billet are tested, including diameter, thickness, roundness, etc., to ensure that the billet quality meets production requirements.

[0030] Heat treatment includes normalizing, quenching and tempering. The normalizing temperature is 920℃ and the holding time is 2h to eliminate the internal stress of the material and improve the organizational structure; the quenching temperature is 840℃ and the holding time is 1h to obtain the required hardness and wear resistance; the tempering temperature is 600℃ and the holding time is 2h to reduce quenching stress and improve the toughness of the material.

[0031] The grinding depth of fine machining is 0.01mm to ensure that the dimensional accuracy and surface roughness of the inner and outer rings of the bearing meet the design requirements. The polishing speed is 2000rpm to remove tiny scratches on the surface and improve the surface finish to ensure that the dimensional accuracy and surface quality meet the design requirements.

[0032] Additives include lubricants, antioxidants and alloying elements. Lubricants help improve the fluidity and compressibility of bearing steel powder, and their mass proportion is between 0.2% and 2%. Antioxidants are used to protect bearing steel powder from oxidation during subsequent processing, and their mass proportion is between 0.1% and 1%. Alloying elements are added according to specific performance requirements, and their mass proportion is between 0.1% and 3%. Alloying elements include carbon, chromium, manganese, silicon, molybdenum, vanadium and titanium. When mixing bearing steel powder with additives, a high-speed mixer is used to ensure the uniformity and stability of the powder. The speed and time should be controlled during mixing to ensure uniform mixing without destroying the original properties of the bearing steel powder. Too high a speed will cause the bearing steel powder to overheat or oxidize, and too long a mixing time will introduce too many impurities. The mixing is completed. Finally, the uniformity of the mixture of bearing steel and additives should be tested. If there is local unevenness or impurities, the mixing parameters should be adjusted or re-mixed in time. Bearing steel powder with added antioxidants should be stored in a dry, ventilated and dust-free environment to prevent moisture, oxidation or contamination. Antioxidants are usually selected to be stable at high temperatures and to form a dense oxide film on the metal surface. For bearing steel powder, commonly used antioxidants include two major categories: organic and inorganic. Inorganic antioxidants include silanes and silicates, and organic antioxidants include polymer compounds. Antioxidants should have low volatility, be able to remain stable during the powder metallurgy process, and not introduce harmful impurities into the material. At the same time, they should also be able to form a continuous and dense oxide film on the surface of the bearing steel to effectively prevent the intrusion of oxygen.

[0033] Among them, carbon is used to improve the hardness and strength of bearing steel, with a content of 0.95-1.10%; chromium is used to improve the wear resistance, corrosion resistance and hardness of bearing steel, with a content of 1.45-1.75%; manganese is used to improve the strength, hardness and toughness of bearing steel, with a content of 0.25-0.50%; silicon is used to improve the strength and hardness of bearing steel, with a content of 0.15-0.35%; molybdenum is used to improve the hardness, wear resistance and toughness of bearing steel, with a content of 0.15-0.30%; vanadium is used to refine the grains of bearing steel and improve strength and toughness, with a content of 0.05-0.20%; titanium is used to improve the corrosion resistance and wear resistance of bearing steel, with a content of 0.01-0.10%.

[0034] In addition, there are some other elements, such as nickel, copper, aluminum, etc., which are added to bearing steel according to specific needs to improve its performance. The content of these alloy elements is generally low, but they have an important influence on the performance of bearing steel.

[0035] It should be noted that in order to verify the basic feasibility of the blank making method provided in the embodiment of the present application, the basic performance of the blank making method provided in the embodiment of the present application is understood through the evaluation of the finished product. Therefore, the evaluation benchmark is set, the inner and outer diameters need to reach IT6-IT8, and 5-15μm is taken, which is qualified within this range; the surface roughness Ra0.4μm-Ra1.6μm is qualified within this range; the material utilization rate reaches 70%-80%, which is qualified within this range.

[0036] Comparative Example

[0037] Select high-purity bearing steel, put the bearing steel into the forging equipment, heat it to the forging temperature of 1200℃, and then forge it. Each forging time is 60s and the forging pressure is 500T to form the preliminary shape of the inner and outer rings of the bearing. The inner and outer rings of the bearing are heat treated with a normalizing temperature of 920℃ and a holding time of 2h; a quenching temperature of 840℃ and a holding time of 1h; a tempering temperature of 600℃ and a holding time of 2h; the inner and outer rings of the bearing after heat treatment are fine-machined with a grinding depth of 0.01mm and a polishing speed of 2000rpm. The dimensional accuracy, surface roughness and material utilization rate of the finished product are evaluated. The inner and outer diameter accuracy is 20μm, the surface roughness Ra is 1.8μm, and the material utilization rate is 65%.

[0038] Experimental Example 1

[0039] High-purity bearing steel powder was selected and mixed with additives at a mass ratio of 98:2. The mixed bearing steel powder was put into a mold and pressed at 250 MPa for 30 seconds by isostatic pressing technology to form a billet. The pressed billet was put into a warm composite extruder, the extrusion temperature was controlled to reach 1100°C, and the billet was extruded at a speed of 10 mm / s to cause plastic deformation of the billet to form the required inner and outer ring shapes of the bearing. The extruded inner and outer rings of the bearing were heat treated at a normalizing temperature of 920°C and a holding time of 2 h; the quenching temperature was 840°C and a holding time of 1 h; the tempering temperature was 600°C and a holding time of 2 h; the inner and outer rings of the bearing after heat treatment were fine-machined with a grinding depth of 0.01 mm and a polishing speed of 3000 rpm. The dimensional accuracy, surface roughness and material utilization rate of the processed product were evaluated, and the inner and outer diameter accuracy was 6.3 μm, the surface roughness Ra was 0.52 μm, and the material utilization rate was 86%.

[0040] Experimental Example 2

[0041] High-purity bearing steel powder was selected and mixed with additives at a mass ratio of 98:2. The mixed bearing steel powder was put into a mold and pressed at 250 MPa for 30 seconds by isostatic pressing technology to form a billet. The pressed billet was put into a warm composite extruder, the extrusion temperature was controlled to reach 1100°C, and the billet was extruded at a speed of 9 mm / s to cause plastic deformation of the billet to form the required shape of the inner and outer rings of the bearing. The extruded inner and outer rings of the bearing were heat treated with a normalizing temperature of 920°C and a holding time of 2h; a quenching temperature of 840°C and a holding time of 1h; a tempering temperature of 600°C and a holding time of 2h; the inner and outer rings of the bearing after heat treatment were fine-machined with a grinding depth of 0.01mm and a polishing speed of 3000rpm. The dimensional accuracy, surface roughness and material utilization rate of the processed product were evaluated, and the inner and outer diameter accuracy was 8.5μm, the surface roughness Ra0.58μm, and the material utilization rate was 85%.

[0042] Experimental Example 3

[0043] High-purity bearing steel powder was selected and mixed with additives at a mass ratio of 98:2. The mixed bearing steel powder was put into a mold and pressed at 250 MPa for 30 seconds by isostatic pressing technology to form a billet. The pressed billet was put into a warm composite extruder, the extrusion temperature was controlled to reach 1100°C, and the billet was extruded at a speed of 8 mm / s to cause plastic deformation of the billet to form the required inner and outer ring shapes of the bearing. The extruded inner and outer rings of the bearing were heat treated with a normalizing temperature of 920°C and a holding time of 2h; a quenching temperature of 840°C and a holding time of 1h; a tempering temperature of 600°C and a holding time of 2h; the inner and outer rings of the bearing after heat treatment were fine-machined with a grinding depth of 0.01mm and a polishing speed of 3000rpm. The dimensional accuracy, surface roughness and material utilization rate of the processed product were evaluated, and the inner and outer diameter accuracy was 9.4μm, the surface roughness Ra0.61μm, and the material utilization rate was 85%.

[0044] Experimental Example 4

[0045] High-purity bearing steel powder was selected and mixed with additives at a mass ratio of 98:2. The mixed bearing steel powder was put into a mold and pressed at 250 MPa for 30 seconds by isostatic pressing technology to form a billet. The pressed billet was put into a warm composite extruder, the extrusion temperature was controlled to reach 1050°C, and the billet was extruded at a speed of 10 mm / s to cause plastic deformation of the billet to form the required inner and outer ring shapes of the bearing. The extruded inner and outer rings of the bearing were heat treated at a normalizing temperature of 920°C and a holding time of 2 h; the quenching temperature was 840°C and a holding time of 1 h; the tempering temperature was 600°C and a holding time of 2 h; the inner and outer rings of the bearing after heat treatment were fine-machined with a grinding depth of 0.01 mm and a polishing speed of 3000 rpm. The dimensional accuracy, surface roughness and material utilization rate of the processed product were evaluated, and the inner and outer diameter accuracy was 7.4 μm, the surface roughness Ra was 0.58 μm, and the material utilization rate was 85%.

[0046] Experimental Example 5

[0047] High-purity bearing steel powder was selected and mixed with additives at a mass ratio of 98:2. The mixed bearing steel powder was put into a mold and pressed at 250 MPa for 30 seconds by isostatic pressing technology to form a billet. The pressed billet was put into a warm composite extruder, the extrusion temperature was controlled to reach 1000°C, and the billet was extruded at a speed of 10 mm / s to cause plastic deformation of the billet to form the required inner and outer ring shapes of the bearing. The extruded inner and outer rings of the bearing were heat treated at a normalizing temperature of 920°C and a holding time of 2 h; the quenching temperature was 840°C and a holding time of 1 h; the tempering temperature was 600°C and a holding time of 2 h; the inner and outer rings of the bearing after heat treatment were fine-machined with a grinding depth of 0.01 mm and a polishing speed of 3000 rpm. The dimensional accuracy, surface roughness and material utilization rate of the processed product were evaluated, and the inner and outer diameter accuracy was 8.2 μm, the surface roughness Ra was 0.63 μm, and the material utilization rate was 85%.

[0048] Experimental Example 6

[0049] Conventional bearing steel powder was selected and mixed with additives at a mass ratio of 98:2. The mixed bearing steel powder was put into a mold and pressed at 250 MPa for 30 seconds by isostatic pressing technology to form a billet. The pressed billet was put into a warm composite extruder, the extrusion temperature was controlled to reach 1100°C, and the billet was extruded at a speed of 10 mm / s to cause plastic deformation of the billet to form the required inner and outer ring shapes of the bearing. The extruded inner and outer rings of the bearing were heat treated with a normalizing temperature of 920°C and a holding time of 2 h; a quenching temperature of 840°C and a holding time of 1 h; a tempering temperature of 600°C and a holding time of 2 h. The inner and outer rings of the bearing after heat treatment were finely processed with a grinding depth of 0.01 mm and a polishing speed of 3000 rpm. The dimensional accuracy, surface roughness and material utilization rate of the processed product were evaluated, and the inner and outer diameter accuracy was 11.4 μm, the surface roughness Ra was 1.45 μm, and the material utilization rate was 65%.

[0050] Experimental Example 7

[0051] Alloy bearing steel powder was selected and mixed with additives at a mass ratio of 98:2. The mixed bearing steel powder was put into a mold and pressed at 250 MPa for 30 seconds by isostatic pressing technology to form a billet. The pressed billet was put into a warm composite extruder, the extrusion temperature was controlled to reach 1100°C, and the billet was extruded at a speed of 10 mm / s to cause plastic deformation of the billet to form the required inner and outer ring shapes of the bearing. The extruded inner and outer rings of the bearing were heat treated at a normalizing temperature of 920°C and a holding time of 2 h; the quenching temperature was 840°C and a holding time of 1 h; the tempering temperature was 600°C and a holding time of 2 h; the inner and outer rings of the bearing after heat treatment were finely processed with a grinding depth of 0.01 mm and a polishing speed of 3000 rpm. The dimensional accuracy, surface roughness and material utilization rate of the processed product were evaluated, and the inner and outer diameter accuracy was 7.6 μm, the surface roughness Ra was 0.67 μm, and the material utilization rate was 74%.

[0052] It can be seen that the comparative example, as a traditional forging method, has low dimensional accuracy, surface roughness and material utilization rate of the product after processing; Experimental Example 1 is used as a basic parameter experiment to compare with the comparative example to verify the correctness of the blank making method of the inner and outer rings of the bearing steel of this embodiment.

[0053] It can be seen from Experimental Examples 2 and 3 that, on the basis of Experimental Example 1, the extrusion speed is adjusted, and the dimensional accuracy, surface roughness and material utilization rate of the processed product are reduced, indicating that if the extrusion speed is lower than 10 mm / s, the dimensional accuracy, surface roughness and material utilization rate of the processed product will be reduced.

[0054] It can be seen from Experimental Examples 4 and 5 that, on the basis of Experimental Example 1, the extrusion temperature is adjusted, and the dimensional accuracy, surface roughness and material utilization rate of the processed product are reduced, indicating that when the extrusion temperature is lower than 1100°C, the dimensional accuracy, surface roughness and material utilization rate of the processed product will be reduced.

[0055] It can be seen from Experimental Examples 6 and 7 that, based on Experimental Example 1, the material of the bearing steel powder was adjusted, and the dimensional accuracy, surface roughness and material utilization rate of the processed product were reduced, indicating that the purity of the bearing steel powder will affect the dimensional accuracy, surface roughness and material utilization rate of the product.

[0056] This specific embodiment is merely an explanation of the invention and is not a limitation of the invention. After reading this specification, those skilled in the art may make non-creative modifications to this embodiment as needed. However, as long as they are within the scope of protection of the invention, they are protected by patent law.

Claims

1. A method for manufacturing inner and outer rings of a bearing, characterized in that: The following steps are involved: S1. Select high-purity bearing steel powder and mix it with additives in a mass ratio of 95:5-98:2; S2, putting the mixed bearing steel powder into a mold, and pressing it at 250-300 MPa for 60 seconds by isostatic pressing technology to form a blank; S3. Place the pressed billet into a warm composite extruder, control the extrusion temperature to 1100±5°C, and extrude at a speed of 10±0.1mm / s to cause the billet to undergo plastic deformation to form the required inner and outer ring shapes of the bearing; S4. Heat treatment is performed on the extruded inner and outer rings of the bearing to improve the structure and performance of the material; S5. Finish the inner and outer rings of the bearing after heat treatment to ensure that their dimensional accuracy and surface quality meet the requirements; Wherein, the heat treatment includes normalizing, quenching and tempering; The normalizing temperature is 920°C and the holding time is 2h; The quenching temperature is 840°C and the holding time is 1h; The tempering temperature is 600° C. and the holding time is 2 h.

2. The method for manufacturing inner and outer rings of a bearing according to claim 1, characterized in that: The precision of the mold is ±0.01 mm, and the surface roughness is less than Ra0.8 μm.

3. The method for manufacturing inner and outer rings of a bearing according to claim 1, characterized in that: The grinding depth of the finishing process is 0.01 mm, and the polishing speed is 2000 rpm.

4. The method for manufacturing inner and outer rings of a bearing according to claim 1, characterized in that: The additives include lubricants, antioxidants and alloying elements including carbon, chromium, manganese, silicon, molybdenum, vanadium and titanium.