Winding flat wire for explosion-proof motor and manufacturing method thereof
Through the treatment methods of glue modifier and paint improvement fluid, the problem of poor insulation performance of flat wire windings is solved, the heat resistance and water resistance stability are significantly improved, and the use efficiency of winding flat wires for explosion-proof motors is improved.
Patent Information
- Application Number
- CN202411053497.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2044-08-02
AI Technical Summary
The existing flat wire windings used in explosion-proof motors have poor insulation performance and insufficient heat and water resistance stability, which limits the efficiency of the product.
Adopt glue modifier and paint improvement liquid treatment method, including immersing the rectangular body in the glue modifier and wrapping it with double layers of polyimide film and glass fiber, and then ultrasonic treatment in the paint improvement liquid to coordinate the glue modification The synergistic effect of agent and paint improvement fluid enhances insulation and stability.
It significantly improves the insulation, heat resistance and waterproof stability of the winding rectangular wire, and improves the efficiency of the product.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sintered winding flat wires, and in particular to a winding flat wire for an explosion-proof motor and a manufacturing method thereof. Background Art
[0002] The flat wire windings used in explosion-proof motors have the advantages of high slot fill rate, high power density, and good temperature performance. In the design and manufacture of flat wire motors, there are different winding arrangements, which will have a direct impact on the complexity of stator manufacturing; the existing winding flat wires have poor insulation performance, and the product's heat and water resistance are poor, which limits the product's efficiency. Summary of the invention
[0003] In view of the defects of the prior art, the purpose of the present invention is to provide a winding flat wire for an explosion-proof motor and a manufacturing method thereof, so as to solve the problems raised in the above background technology.
[0004] The present invention solves the technical problem by adopting the following technical solution:
[0005] The present invention provides a method for manufacturing a flat winding wire for an explosion-proof motor, comprising the following steps:
[0006] Step 1: immerse the flat wire into the glue modifier for immersion treatment, the immersion pressure is 10-20MPa, the immersion time is 10-15min, and the immersion is completed and dried;
[0007] Step 2: Wrap the dried flat wire with a double-layer polyimide film, wrapping two layers, and the thickness of a single layer of the polyimide film is 0.01-0.02 mm;
[0008] Step 3, then wrapping the glass fibers, the glass fibers are wrapped in two layers in opposite directions to obtain a glass fiber wrapping layer;
[0009] Step 4, subjecting the glass fiber coating to ultrasonic treatment in the paint improvement liquid, and after the adjustment, drying, a winding flat wire can be obtained; the preparation method of the adhesive modifier is:
[0010] Blend 10-15 parts of phenolic adhesive resin, 2-5 parts of isocyanate and 1-2 parts of silane coupling agent KH560, then add 1-3 parts of chitosan solution, continue to mix thoroughly, and obtain a gum base agent;
[0011] The bentonite is first heat-treated at 210-230°C for 5-10 minutes, then cooled to 55°C at a rate of 2-5°C / min, and kept warm. 4-7 parts of the heat-insulating bentonite, 1-3 parts of nano-silica sol, 2-5 parts of yttrium nitrate solution and 1-2 parts of graphene modifier are mixed and ball-milled at a ball-milling speed of 1500r / min for 2h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a bentonite agent. The bentonite agent and the gum base agent are fully mixed at a weight ratio of 2:7 to obtain a gum modifier. The preparation method of the paint improvement liquid is as follows:
[0012] Heat 20-25 parts of phenolic epoxy resin until it is melted, then add it into 30-40 parts of bisphenol A epoxy resin solution and stir evenly to dissolve it, then add 4-7 parts of glass fiber agent and 2-5 parts of thiol ester curing agent and mix thoroughly to obtain a paint improvement solution.
[0013] Preferably, the ultrasonic power of the ultrasonic treatment is adjusted to 350-400W, and the ultrasonic time is 20min.
[0014] Preferably, the mass fraction of the yttrium nitrate solution is 2-5%; the mass fraction of the chitosan solution is 4-7%.
[0015] Preferably, the preparation method of the graphene modifier is:
[0016] The graphene is added to a 5% by mass sodium silicate solution in a weight ratio of 2:5 and ultrasonically mixed to obtain graphene adjusted with sodium silicate. 4-7 parts of the graphene adjusted with sodium silicate, 2-5 parts of sodium lignin sulfonate solution, 1-2 parts of stearic acid and 3-5 parts of yttrium oxide are mixed and ball-milled at a ball-milling speed of 1000-1500 r / min for 1 hour. After the ball-milling is completed, the mixture is washed with water and dried to obtain a graphene modifier.
[0017] Preferably, the mass fraction of the sodium lignin sulfonate solution is 10-15%.
[0018] Preferably, the bisphenol A epoxy resin solution is prepared by mixing bisphenol A epoxy resin, xylene and n-butanol in a weight ratio of 3:2:1.
[0019] Preferably, the glass fiber agent is prepared by mixing glass fiber with a sufficient amount of 5% by mass sodium alginate solution, and then washing and drying to obtain the glass fiber agent.
[0020] The invention also provides a method for manufacturing a winding flat wire for an explosion-proof motor, and manufactures the winding flat wire for the explosion-proof motor.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] In the method for making the winding flat wire of the present invention, the flat wire body is first immersed in a glue modifier, and then wrapped with a double-layer polyimide film and a glass fiber, and then ultrasonic treatment is adjusted in a paint improvement liquid. The paint improvement liquid and the glue modifier are coordinated and synergistically formulated to enhance the insulation of the product and improve the heat resistance and waterproof stability of the product. DETAILED DESCRIPTION
[0023] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in conjunction with specific embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] A method for manufacturing a flat winding wire for an explosion-proof motor according to the present embodiment comprises the following steps:
[0025] Step 1: immerse the flat wire into the glue modifier for immersion treatment, the immersion pressure is 10-20MPa, the immersion time is 10-15min, and the immersion is completed and dried;
[0026] Step 2: Wrap the dried flat wire with a double-layer polyimide film, wrapping two layers, and the thickness of a single layer of the polyimide film is 0.01-0.02 mm;
[0027] Step 3, then wrapping the glass fibers, the glass fibers are wrapped in two layers in opposite directions to obtain a glass fiber wrapping layer;
[0028] Step 4: subjecting the glass fiber coating to ultrasonic treatment in the paint improving liquid, and after the conditioning is completed, drying is performed to obtain the winding flat wire.
[0029] The ultrasonic power of the ultrasonic treatment in this embodiment is adjusted to 350-400W, and the ultrasonic time is 20min.
[0030] The preparation method of the glue modifier of this embodiment is:
[0031] Blend 10-15 parts of phenolic adhesive resin, 2-5 parts of isocyanate and 1-2 parts of silane coupling agent KH560, then add 1-3 parts of chitosan solution, continue to mix thoroughly, and obtain a gum base agent;
[0032] The bentonite is first heat-treated at 210-230°C for 5-10 min, then the temperature is reduced to 55°C at a rate of 2-5°C / min and kept warm. 4-7 parts of the heat-insulated bentonite, 1-3 parts of nano-silica sol, 2-5 parts of yttrium nitrate solution and 1-2 parts of graphene modifier are blended and ball-milled at a speed of 1500r / min for 2h. After the ball milling is completed, the mixture is washed with water and dried to obtain a bentonite agent. The bentonite agent and the gum base agent are fully mixed in a weight ratio of 2:7 to obtain a gum modifier.
[0033] The mass fraction of the yttrium nitrate solution in this embodiment is 2-5%; the mass fraction of the chitosan solution is 4-7%.
[0034] The preparation method of the graphene modifier of this embodiment is:
[0035] The graphene is added to a 5% by mass sodium silicate solution in a weight ratio of 2:5 and ultrasonically mixed to obtain graphene adjusted with sodium silicate. 4-7 parts of the graphene adjusted with sodium silicate, 2-5 parts of sodium lignin sulfonate solution, 1-2 parts of stearic acid and 3-5 parts of yttrium oxide are mixed and ball-milled at a ball-milling speed of 1000-1500 r / min for 1 hour. After the ball-milling is completed, the mixture is washed with water and dried to obtain a graphene modifier.
[0036] The mass fraction of the sodium lignin sulfonate solution in this embodiment is 10-15%.
[0037] The preparation method of the paint improving liquid of the present embodiment is:
[0038] Heat 20-25 parts of phenolic epoxy resin until it is melted, then add it into 30-40 parts of bisphenol A epoxy resin solution and stir evenly to dissolve it, then add 4-7 parts of glass fiber agent and 2-5 parts of thiol ester curing agent and mix thoroughly to obtain a paint improvement solution.
[0039] The bisphenol A epoxy resin solution of this embodiment is prepared by mixing bisphenol A epoxy resin, xylene and n-butanol in a weight ratio of 3:2:1.
[0040] The glass fiber agent of this embodiment is obtained by mixing glass fibers with a sufficient amount of sodium alginate solution with a mass fraction of 5%, and then washing and drying.
[0041] The present embodiment provides a method for manufacturing a flat winding wire for an explosion-proof motor, and manufactures a flat winding wire for an explosion-proof motor. Example 1
[0042] A method for manufacturing a flat winding wire for an explosion-proof motor according to the present embodiment comprises the following steps:
[0043] Step 1: immerse the flat wire into the glue modifier for immersion treatment, the immersion pressure is 10MPa, the immersion time is 10min, the immersion is completed, and the wire is dried;
[0044] Step 2: Wrap the dried flat wire with a double-layer polyimide film, wrapping two layers, and the thickness of a single layer of the polyimide film is 0.01 mm;
[0045] Step 3, then wrapping the glass fibers, the glass fibers are wrapped in two layers in opposite directions to obtain a glass fiber wrapping layer;
[0046] Step 4: subjecting the glass fiber coating to ultrasonic treatment in the paint improving liquid, and after the conditioning is completed, drying is performed to obtain the winding flat wire.
[0047] The ultrasonic power of the ultrasonic treatment in this embodiment is 350W, and the ultrasonic time is 20min.
[0048] The preparation method of the glue modifier of this embodiment is:
[0049] 10 parts of phenolic adhesive resin, 2 parts of isocyanate and 1 part of silane coupling agent KH560 were mixed, and then 1 part of chitosan solution was added, and the mixture was mixed thoroughly to obtain a gum base agent;
[0050] The bentonite was first heat treated at 210°C for 5 min, then the temperature was reduced to 55°C at a rate of 2°C / min and kept warm. 4 parts of heat-insulated bentonite, 1 part of nano-silica sol, 2 parts of yttrium nitrate solution and 1 part of graphene modifier were blended and ball-milled at a speed of 1500r / min for 2h. After the ball milling was completed, the mixture was washed with water and dried to obtain a bentonite agent. The bentonite agent and the gum base agent were fully mixed in a weight ratio of 2:7 to obtain a gum modifier.
[0051] The mass fraction of the yttrium nitrate solution in this embodiment is 2%; the mass fraction of the chitosan solution is 4%.
[0052] The preparation method of the graphene modifier of this embodiment is:
[0053] Graphene was added into a 5% by mass sodium silicate solution in a weight ratio of 2:5 and ultrasonically mixed thoroughly. After mixing, graphene adjusted with sodium silicate was obtained. 4 parts of graphene adjusted with sodium silicate, 2 parts of sodium lignin sulfonate solution, 1 part of stearic acid and 3 parts of yttrium oxide were blended and ball-milled at a ball-milling speed of 1000 r / min for 1 hour. After ball-milling, the mixture was washed with water and dried to obtain a graphene modifier.
[0054] The mass fraction of the sodium lignin sulfonate solution in this embodiment is 10%.
[0055] The preparation method of the paint improving liquid of the present embodiment is:
[0056] 20 parts of phenolic epoxy resin are first heated to melt, then added into 30 parts of bisphenol A epoxy resin solution and stirred evenly to dissolve, followed by adding 4 parts of glass fiber agent and 2 parts of thiol ester curing agent and blending thoroughly to obtain a paint improvement solution.
[0057] The bisphenol A epoxy resin solution of this embodiment is prepared by mixing bisphenol A epoxy resin, xylene and n-butanol in a weight ratio of 3:2:1.
[0058] The glass fiber agent of this embodiment is obtained by mixing glass fibers with a sufficient amount of sodium alginate solution with a mass fraction of 5%, and then washing and drying.
[0059] The present embodiment provides a method for manufacturing a flat winding wire for an explosion-proof motor, and manufactures a flat winding wire for an explosion-proof motor. Example 2
[0060] A method for manufacturing a flat winding wire for an explosion-proof motor according to the present embodiment comprises the following steps:
[0061] Step 1: immerse the flat wire into the glue modifier for immersion treatment, the immersion pressure is 20MPa, the immersion time is 15min, the immersion is completed, and the wire is dried;
[0062] Step 2: Wrap the dried flat wire with a double-layer polyimide film, wrapping two layers, and the thickness of a single layer of the polyimide film is 0.02 mm;
[0063] Step 3, then wrapping the glass fibers, the glass fibers are wrapped in two layers in opposite directions to obtain a glass fiber wrapping layer;
[0064] Step 4: subjecting the glass fiber coating to ultrasonic treatment in the paint improving liquid, and after the conditioning is completed, drying is performed to obtain the winding flat wire.
[0065] The ultrasonic power of the ultrasonic treatment in this embodiment is 400 W, and the ultrasonic time is 20 min.
[0066] The preparation method of the glue modifier of this embodiment is:
[0067] 15 parts of phenolic adhesive resin, 5 parts of isocyanate and 2 parts of silane coupling agent KH560 were mixed, and then 3 parts of chitosan solution were added, and the mixture was mixed thoroughly to obtain a gum base agent;
[0068] The bentonite was first heat treated at 230°C for 10 min, then the temperature was reduced to 55°C at a rate of 5°C / min and kept warm. 7 parts of heat-insulated bentonite, 3 parts of nano-silica sol, 5 parts of yttrium nitrate solution and 2 parts of graphene modifier were blended and ball-milled at a speed of 1500r / min for 2h. After the ball milling was completed, the mixture was washed with water and dried to obtain a bentonite agent. The bentonite agent and the gum base agent were fully mixed in a weight ratio of 2:7 to obtain a gum modifier.
[0069] The mass fraction of the yttrium nitrate solution in this embodiment is 5%; the mass fraction of the chitosan solution is 7%.
[0070] The preparation method of the graphene modifier of this embodiment is:
[0071] Graphene was added into a 5% by mass sodium silicate solution in a weight ratio of 2:5 and ultrasonically mixed thoroughly. After mixing, graphene adjusted with sodium silicate was obtained. 7 parts of graphene adjusted with sodium silicate, 5 parts of sodium lignin sulfonate solution, 2 parts of stearic acid and 5 parts of yttrium oxide were blended and ball-milled at a ball-milling speed of 1500 r / min for 1 hour. After ball-milling, the mixture was washed with water and dried to obtain a graphene modifier.
[0072] The mass fraction of the sodium lignin sulfonate solution in this embodiment is 15%.
[0073] The preparation method of the paint improving liquid of the present embodiment is:
[0074] 25 parts of phenolic epoxy resin are first heated to melt, then added into 40 parts of bisphenol A epoxy resin solution and stirred evenly to dissolve, and then 7 parts of glass fiber agent and 5 parts of thiol ester curing agent are added and mixed thoroughly to obtain a paint improvement liquid.
[0075] The bisphenol A epoxy resin solution of this embodiment is prepared by mixing bisphenol A epoxy resin, xylene and n-butanol in a weight ratio of 3:2:1.
[0076] The glass fiber agent of this embodiment is obtained by mixing glass fibers with a sufficient amount of sodium alginate solution with a mass fraction of 5%, and then washing and drying.
[0077] The present embodiment provides a method for manufacturing a flat winding wire for an explosion-proof motor, and manufactures a flat winding wire for an explosion-proof motor. Example 3
[0078] A method for manufacturing a flat winding wire for an explosion-proof motor according to the present embodiment comprises the following steps:
[0079] Step 1: immerse the flat wire into the glue modifier for immersion treatment, the immersion pressure is 15MPa, the immersion time is 12.5min, the immersion is completed, and the wire is dried;
[0080] Step 2: Wrap the dried flat wire with a double-layer polyimide film, wrapping two layers, and the thickness of a single layer of the polyimide film is 0.015 mm;
[0081] Step 3, then wrapping the glass fibers, the glass fibers are wrapped in two layers in opposite directions to obtain a glass fiber wrapping layer;
[0082] Step 4: subjecting the glass fiber coating to ultrasonic treatment in the paint improving liquid, and after the conditioning is completed, drying is performed to obtain the winding flat wire.
[0083] The ultrasonic power of the ultrasonic treatment in this embodiment is 370W, and the ultrasonic time is 20min.
[0084] The preparation method of the glue modifier of this embodiment is:
[0085] 12.5 parts of phenolic adhesive resin, 3.5 parts of isocyanate and 1.5 parts of silane coupling agent KH560 were mixed, and then 2 parts of chitosan solution were added, and the mixture was mixed thoroughly to obtain a gum base agent;
[0086] The bentonite was first heat treated at 220°C for 7.5 min, then the temperature was reduced to 55°C at a rate of 3.5°C / min and kept warm. 5.5 parts of heat-insulated bentonite, 2 parts of nano-silica sol, 3.5 parts of yttrium nitrate solution and 1.5 parts of graphene modifier were blended and ball-milled at a speed of 1500 r / min for 2 h. After the ball milling was completed, the mixture was washed with water and dried to obtain a bentonite agent. The bentonite agent and the gum base agent were fully mixed in a weight ratio of 2:7 to obtain a gum modifier.
[0087] The mass fraction of the yttrium nitrate solution in this embodiment is 3.5%; the mass fraction of the chitosan solution is 5.5%.
[0088] The preparation method of the graphene modifier of this embodiment is:
[0089] Graphene was added into a 5% by mass sodium silicate solution in a weight ratio of 2:5 and ultrasonically mixed thoroughly. After mixing, graphene adjusted with sodium silicate was obtained. 5.5 parts of graphene adjusted with sodium silicate, 3.5 parts of sodium lignin sulfonate solution, 1.5 parts of stearic acid and 4 parts of yttrium oxide were blended and ball-milled at a ball-milling speed of 1250 r / min for 1 hour. After ball-milling, the mixture was washed with water and dried to obtain a graphene modifier.
[0090] The mass fraction of the sodium lignin sulfonate solution in this embodiment is 12.5%.
[0091] The preparation method of the paint improving liquid of the present embodiment is:
[0092] 22.5 parts of phenolic epoxy resin are first heated to melt, then added to 35 parts of bisphenol A epoxy resin solution and stirred evenly to dissolve, followed by adding 5.5 parts of glass fiber agent and 3.5 parts of thiol ester curing agent and blending thoroughly to obtain a paint improvement solution.
[0093] The bisphenol A epoxy resin solution of this embodiment is prepared by mixing bisphenol A epoxy resin, xylene and n-butanol in a weight ratio of 3:2:1.
[0094] The glass fiber agent of this embodiment is obtained by mixing glass fibers with a sufficient amount of sodium alginate solution with a mass fraction of 5%, and then washing and drying.
[0095] The present embodiment provides a method for manufacturing a flat winding wire for an explosion-proof motor, and manufactures a flat winding wire for an explosion-proof motor.
[0096] Comparative Example 1
[0097] The difference from Example 3 is that no rubber modifier is added.
[0098] Comparative Example 2
[0099] The difference from Example 3 is that no bentonite agent is added to the rubber modifier.
[0100] Comparative Example 3
[0101] The difference from Example 3 is that no graphene modifier is added to the bentonite agent.
[0102] Comparative Example 4
[0103] Different from Example 3, graphene is used instead of graphene in the graphene modifier.
[0104] Comparative Example 5
[0105] The difference from Example 3 is that no paint improvement liquid treatment is added.
[0106] The product performances of Examples 1-3 and Comparative Examples 1-5 of the present invention were tested, and the test results are as follows.
[0107]
[0108] It can be seen from Examples 1-3 and Comparative Examples 1-5 that the products of Examples 1-3 of the present invention have excellent insulation, and the products have significant water resistance and heat stability effects. The products are not treated with glue modifiers or paint improvement liquid, and the product performance effect is significantly deteriorated. In addition, when no bentonite is added to the glue modifier, graphene modifier is added to the bentonite agent, or graphene is used as a substitute in the graphene modifier, the product performance tends to deteriorate. Only when the product raw materials are obtained by the method of the present invention, the product performance effect is most significant, and the effects of other methods are not as obvious as those of the present invention.
[0109] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above and that the present invention can be implemented in other specific forms without departing from the spirit or essential features of the present invention. Therefore, the embodiments should be considered exemplary and non-restrictive in all respects, and the scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims be included in the present invention.
[0110] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A method for manufacturing a flat winding wire for an explosion-proof motor, characterized in that: The following steps are involved: Step 1: immerse the flat wire into the glue modifier for immersion treatment, the immersion pressure is 10-20MPa, the immersion time is 10-15min, and the immersion is completed and dried; Step 2: Wrap the dried flat wire with a double-layer polyimide film, wrapping two layers, and the thickness of a single layer of the polyimide film is 0.01-0.02 mm; Step 3, then wrapping the glass fibers, the glass fibers are wrapped in two layers in opposite directions to obtain a glass fiber wrapping layer; Step 4, subjecting the glass fiber coating to ultrasonic treatment in the paint improvement liquid, and after the adjustment, drying, a winding flat wire can be obtained; the preparation method of the adhesive modifier is: Blend 10-15 parts of phenolic adhesive resin, 2-5 parts of isocyanate and 1-2 parts of silane coupling agent KH560, then add 1-3 parts of chitosan solution, continue to mix thoroughly, and obtain a gum base agent; The bentonite is first heat treated at 210-230°C for 5-10 minutes, then the temperature is reduced to 55°C at a rate of 2-5°C / min, and the temperature is kept warm. 4-7 parts of the heat-insulated bentonite, 1-3 parts of nano-silica sol, 2-5 parts of yttrium nitrate solution and 1-2 parts of graphene modifier are mixed and ball-milled at a ball-milling speed of 1500r / min for 2h. After the ball-milling is completed, the mixture is washed with water and dried to obtain a bentonite agent. The bentonite agent and the gum base agent are fully mixed at a weight ratio of 2:7 to obtain a gum modifier. The preparation method of the paint improvement liquid is: 20-25 parts of phenolic epoxy resin are first heated to melt, then added to 30-40 parts of bisphenol A epoxy resin solution and stirred evenly to dissolve, and then 4-7 parts of glass fiber agent and 2-5 parts of mercaptan ester curing agent are added and mixed sufficiently to obtain a paint improvement liquid; The preparation method of the graphene modifier is: The graphene is added to a 5% by mass sodium silicate solution in a weight ratio of 2:5 and ultrasonically mixed to obtain graphene adjusted with sodium silicate. 4-7 parts of the graphene adjusted with sodium silicate, 2-5 parts of sodium lignin sulfonate solution, 1-2 parts of stearic acid and 3-5 parts of yttrium oxide are mixed and ball-milled at a ball-milling speed of 1000-1500 r / min for 1 hour. After the ball-milling is completed, the mixture is washed with water and dried to obtain a graphene modifier.
2. The method for manufacturing a flat winding wire for an explosion-proof motor according to claim 1, characterized in that: The ultrasonic power of the ultrasonic treatment is adjusted to 350-400W, and the ultrasonic time is 20 minutes.
3. The method for manufacturing a flat winding wire for an explosion-proof motor according to claim 1, characterized in that: The mass fraction of the yttrium nitrate solution is 2-5%; the mass fraction of the chitosan solution is 4-7%.
4. The method for manufacturing a flat winding wire for an explosion-proof motor according to claim 1, characterized in that: The mass fraction of the sodium lignin sulfonate solution is 10-15%.
5. The method for manufacturing a flat winding wire for an explosion-proof motor according to claim 1, characterized in that: The bisphenol A epoxy resin solution is prepared by mixing bisphenol A epoxy resin, xylene and n-butanol in a weight ratio of 3:2:
1.
6. The method for manufacturing a flat winding wire for an explosion-proof motor according to claim 5, characterized in that: The glass fiber agent is prepared by mixing glass fiber with a sufficient amount of sodium alginate solution with a mass fraction of 5%, and then washing and drying to obtain the glass fiber agent.
7. A flameproof flat wire for explosion-proof motor manufactured by the method for manufacturing flameproof flat wire for explosion-proof motor as claimed in any one of claims 1 to 6.
Citation Information
Patent Citations
Corona-resistant copper flat wire and method for manufacturing same
CN103413599A
Novel graphene modified universal epoxy paint and preparation method thereof
CN107936771A
Polyimide high-temperature-resistant paint for new energy electromagnetic wire and preparation method of polyimide high-temperature-resistant paint
CN117551387A
High-temperature-resistant heat-conducting insulating paint and preparation method thereof
CN117925055A
Modified graphene non-phosphorus sealing agent and preparation method thereof
CN118206913A