A quasi-hemispherical CdZnTe detector with improved full energy peak shape characteristics
By designing a circular anode and annular cathode structure in a quasi-hemispherical CdZnTe detector and optimizing the electric field distribution, the problem of low electric field intensity and weakened weight potential optimization effect in the detector is solved, and the charge collection efficiency and all-round peak-to-peak shape are improved. feature.
Patent Information
- Application Number
- CN202411054831.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-08-02
AI Technical Summary
When optimizing the anode size of a quasi-hemispherical CdZnTe detector is small, it will easily lead to low electric field intensity in the detector or weakening of the weight potential optimization effect, resulting in a decrease in charge collection efficiency and low-energy tailing of the all-energy peak.
Design a quasi-hemispherical CdZnTe detector including a circular anode and a ring cathode. The positive bias applied to the anode is higher than that of the ring electrode. The side ring electrode is connected to the planar electrode and grounded to increase the electric field intensity within the detector volume and optimize Charge collection and transfer process.
It improves the charge collection efficiency of the detector, increases the total energy peak height, improves the peak-to-contrast ratio, reduces the full width of the peak, and improves the accuracy and reliability of energy spectrum analysis.
Smart Images

Figure CN118588778B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of semiconductor devices, and in particular to a quasi-hemispherical CdZnTe detector with improved full-energy peak shape characteristics. Background Art
[0002] With the continuous development of science and technology, the application scope of nuclear radiation detection technology is becoming wider and wider, involving energy, medicine, industry, agriculture, etc. The key to nuclear radiation detection technology is the radiation detector, and the compound semiconductor CdZnTe (cadmium zinc telluride) is one of the most promising radiation detection materials, with good energy resolution, high detection efficiency and can work at room temperature. Since the hole migration ability of CdZnTe material is poor and it is easy to cause low-energy tailing, current research is mostly focused on preparing CdZnTe detectors into single carrier collection devices. Among them, the quasi-hemispherical detector has a simple electrode structure and low preparation cost, and has been widely used in energy spectrum detection.
[0003] The weighted potential field and electrostatic field generated by quasi-hemispherical detectors with different electrode structures determine the charge collection performance of the detector. However, the optimization of the quasi-hemispherical electrode structure is mostly achieved by selecting a suitable anode size to improve the charge collection efficiency, reduce low-energy tailing, and achieve excellent energy resolution and peak-to-comontane ratio (P / C).
[0004] However, although the weight potential optimization effect is good if the anode pixel is too small, this will also lead to low electric field strength in most of the detector volume, slower carrier drift speed, increased probability of capture, and reduced charge collection efficiency at many positions in the detector; and if the anode pixel is too large, although the electric field strength in the detector volume is enhanced, the weight potential optimization effect will be weakened, thereby reducing the contribution of electrons to the induced charge, deteriorating the unipolarity, and resulting in low-energy tailing of the full-energy peak.
[0005] The above contents are only used to assist in understanding the technical solution of the present application and do not constitute an admission that the above contents are prior art. Summary of the invention
[0006] The main purpose of the present application is to provide a quasi-hemispherical CdZnTe detector with improved full-energy peak shape characteristics, and to propose a quasi-hemispherical CdZnTe detector with improved full-energy peak shape characteristics and high charge collection capability.
[0007] To achieve the above-mentioned purpose, the present application provides a quasi-hemispherical CdZnTe detector with improved full-energy peak shape characteristics, comprising: a detector body, an anode and a cathode; wherein the anode is a circular electrode arranged on the top surface of the detector body, and the center of the circle is located at the center of the top surface; the cathode comprises a planar electrode covering the bottom surface of the detector body, a side ring electrode wrapping the side surface of the detector body, and a ring electrode surrounding the anode;
[0008] There is a first distance between the inner ring of the annular electrode and the anode, a second distance between the outer ring of the annular electrode and the side edge of the top surface of the detector body, and an insulating layer is provided between the annular electrode and the top surface of the detector body; the positive bias voltage applied by the anode is higher than the positive bias voltage applied by the annular electrode;
[0009] The side ring electrode is connected to the plane electrode and is grounded to the plane electrode.
[0010] Optionally, the resistivity of the insulating layer is 10 14 Ω•cm and above.
[0011] Optionally, the resistivity of the CdZnTe material used in the detector body is 10 9 Ω•cm or above, and the working leakage current is less than 10nA.
[0012] Optionally, the CdZnTe material is bare 241 Am energy spectrum, and the energy resolution of gamma rays with an energy of 59.5keV is less than 7%.
[0013] Optionally, the positive bias voltage applied to the anode is 1000V, and the positive bias voltage applied to the ring electrode is 500V.
[0014] Optionally, the anode and the cathode are made of any one of gold, indium, silver and aluminum.
[0015] Optionally, the detector body is a rectangular parallelepiped, and the top and bottom surfaces of the rectangular parallelepiped are squares, and the height of the rectangular parallelepiped is 1 / 2 of the side length of the square.
[0016] Optionally, the diameter of the circular electrode is 1 / 10 to 1 / 5 of the side length of the square; the height of the side ring electrode is at least 4 / 5 of the height of the cuboid; the distance from the inner ring of the ring electrode to the center of the top surface is 1 / 8 of the side length of the square, and the distance from the outer ring of the ring electrode to the center of the top surface is 1 / 4 to 3 / 10 of the side length of the square.
[0017] Optionally, the size of the detector body is 10×10×5 mm 3 The diameter of the circular electrode is 1.25 mm; the height of the side ring electrode is 5 mm; the ring electrode is a square ring, the distance from the inner ring of the ring electrode to the center of the top surface is 1.25 mm, and the distance from the outer ring of the ring electrode to the center of the top surface is 3 mm.
[0018] Optionally, the size of the detector body is 10×10×5 mm 3 The diameter of the circular electrode is 2 mm; the height of the side ring electrode is 4 mm; the ring electrode is a circular ring, the distance from the inner ring of the ring electrode to the center of the top surface is 1.25 mm, and the distance from the outer ring of the ring electrode to the center of the top surface is 2.5 mm.
[0019] The present application provides a quasi-hemispherical CdZnTe detector with improved full-energy peak shape characteristics. Under the premise of ensuring that the weight potential of the anode pixel of the quasi-hemispherical detector is optimized, it ensures the effect of optimizing the weight potential of small pixels, increases the electric field strength in most areas within the detector volume, effectively improves the charge collection efficiency of the quasi-hemispherical CdZnTe detector, and improves the full-energy peak shape characteristics, including increasing the full-energy peak height, increasing the peak-to-Compton ratio, and reducing the full width of the peak (FWTM). BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a schematic diagram of the three-dimensional structure of a quasi-hemispherical CdZnTe detector from an oblique upper perspective in one embodiment of the present application;
[0021] Figure 2 This is a schematic diagram of the three-dimensional structure of a quasi-hemispherical CdZnTe detector from an oblique downward perspective in one embodiment of the present application;
[0022] Figure 3 A top view of a quasi-hemispherical CdZnTe detector in one embodiment of the present application;
[0023] Figure 4 This is a schematic diagram of the dimensions of the side ring electrode that completely covers the side of the detector body in one embodiment of the present application;
[0024] Figure 5 In one embodiment of this application 137 Cs energy spectrum comparison chart;
[0025] Figure 6 This is a schematic diagram of the three-dimensional structure of a quasi-hemispherical CdZnTe detector from an oblique upper perspective in another embodiment of the present application;
[0026] Figure 7 This is a schematic diagram of the three-dimensional structure of a quasi-hemispherical CdZnTe detector from an oblique downward perspective in another embodiment of the present application;
[0027] Figure 8 A top view of a quasi-hemispherical CdZnTe detector in another embodiment of the present application;
[0028] Fig. 9 This is a schematic diagram of the dimensions of a side ring electrode that partially covers the side of the detector body in another embodiment of the present application;
[0029] Fig.10 In another embodiment of the present application 137 Cs energy spectrum comparison chart.
[0030] The realization of the purpose, functional features and advantages of this application will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0031] The embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present application, and should not be construed as limiting the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present application.
[0032] In addition, if the descriptions of "first", "second", etc. are involved in this application, they are only used for descriptive purposes (such as for distinguishing the same or similar features), and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in this field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by this application.
[0033] Reference Figure 1 and Figure 2 In one embodiment, a quasi-hemispherical CdZnTe detector with improved full-energy peak shape characteristics is provided, comprising: a detector body, an anode 1 and a cathode; wherein the anode 1 is a circular electrode arranged on the top surface of the detector body, and the center of the circle is located at the center of the top surface; the cathode comprises a plane electrode 2 covering the bottom surface of the detector body, a side ring electrode 3 wrapping the side surface of the detector body, and a ring electrode 4 surrounding the anode 1;
[0034] There is a first spacing 5 between the inner ring of the annular electrode 4 and the anode 1, there is a second spacing 6 between the outer ring of the annular electrode 4 and the side edge of the top surface of the detector body, and an insulating layer 7 is provided between the annular electrode 4 and the top surface of the detector body; the positive bias voltage applied by the anode 1 is higher than the positive bias voltage applied by the annular electrode 4;
[0035] The side ring electrode 3 is connected to the planar electrode 2 and is grounded together with the planar electrode 2 .
[0036] In this embodiment, a quasi-hemispherical CdZnTe crystal with a suitable thickness is selected as a detection material according to the energy detection range of the gamma rays to prepare the detector body.
[0037] Optionally, the length-height ratio and width-height ratio of the entire detector body are both 2, that is, the length and width are equal, and the top and bottom surfaces are both the same square. In fact, the detector body is a cuboid, and the top and bottom surfaces of the cuboid are squares, and the height of the cuboid is 1 / 2 of the side length of the square.
[0038] The anode 1 of the detector is arranged on the top surface of the detector body and is a circular electrode, and the center of the circular electrode is located at the center of the top surface.
[0039] The cathode of the detector includes a planar electrode 2, a side ring electrode 3 and a ring electrode 4, and the planar electrode 2, the side ring electrode 3 and the ring electrode 4 are located in three positions; wherein, the planar electrode 2 is located on and covers the bottom surface of the detector body; the side ring electrode 3 is located on the side of the detector body, and completely or partially wraps the four sides of the detector body (i.e., surrounds the four sides), and the side ring electrode 3 is also connected to the planar electrode 2 and grounded to the planar electrode 2; the ring electrode 4 is located on the top surface of the detector body and surrounds the anode 1.
[0040] There is a first distance 5 between the inner ring of the annular electrode 4 and the anode 1, and a second distance 6 between the outer ring of the annular electrode 4 and the side edge of the top surface of the detector body; and the shape of the annular electrode 4 includes but is not limited to a square ring and a circular ring.
[0041] Furthermore, an insulating layer 7 is provided between the annular electrode 4 and the top surface of the detector body, so as to prevent the annular electrode 4 from directly contacting the top surface of the detector body. The insulating layer 7 may be made of materials including, but not limited to, aluminum oxide and polyethylene.
[0042] When the quasi-hemispherical CdZnTe detector is used, a positive bias is applied to both the anode 1 and the ring electrode 4, and the positive bias applied to the anode 1 is higher than the positive bias applied to the ring electrode 4. This bias configuration helps to form a specific electric field gradient, optimize the charge collection and transfer process, and thus improve the resolution and peak shape characteristics of the full energy peak.
[0043] Optionally, the positive bias voltage applied to the anode 1 is 1000V, and the positive bias voltage applied to the ring electrode 4 is 500V.
[0044] During the operation of the detector, the anode 1 collects the charges generated by the radiation in the CdZnTe crystal; the planar electrode 2 in the cathode covers the bottom surface of the detector body, and can form an electric field with the anode 1 to guide the charges generated from the CdZnTe crystal to move toward the anode 1; the side ring electrode 3 in the cathode surrounds the CdZnTe crystal, which can help adjust the distribution of the electric field, reduce the edge effect, and play an important role in the collection of charges (that is, the side ring electrode 3 extends toward the anode 1 through the planar electrode 2, helping to guide the charges generated from the CdZnTe crystal to move toward the anode 1); the annular electrode 4 in the cathode surrounds the anode 1, and maintains a first distance 5 between the anode 1 and a second distance 6 between the side edge of the top surface of the detector body, which helps to further optimize the electric field structure.
[0045] In one embodiment, the annular electrode on the top surface of the detector can optimize the weighted potential distribution of the anode pixel of the quasi-hemispherical CdZnTe detector, which is more conducive to single electron collection, thereby reducing the low-energy tail of the full-energy peak and the full width of the peak; and the annular electrode pressurization increases the electric field strength in most of the volume of the detector (especially the electric field strength near the bottom and side areas of the detector), reduces the carrier capture probability, improves the charge collection efficiency, and increases the full-energy peak-to-peak count, increases the peak channel address, and greatly improves the peak-to-compton ratio.
[0046] That is, under the premise of ensuring that the weight potential of the anode pixel of the quasi-hemispherical detector is optimized, the effect of weight potential optimization of small pixels is guaranteed, the electric field strength in most areas within the detector volume is increased, and the charge collection efficiency of the quasi-hemispherical CdZnTe detector is effectively improved, thereby improving the full-energy peak shape characteristics, including an increase in the full-energy peak height, an increase in the peak-to-Compton ratio, and a decrease in the full width of the peak (FWTM).
[0047] It can be seen that the hemispherical CdZnTe detector provided in this embodiment has the advantages of high charge collection efficiency and obvious peak shape characteristics of the gamma energy spectrum full energy peak, which helps to improve the accuracy and reliability of energy spectrum analysis of gamma-ray detectors and meet the needs of energy spectrum detection.
[0048] In one embodiment, based on the above embodiment, the resistivity of the insulating layer 7 is 10 14 Ω•cm and above.
[0049] Optionally, the resistivity of the CdZnTe material used in the detector body is 10 9 Ω•cm or above, the working leakage current is less than 10nA, there are no macro defects and grain boundaries inside the crystal, and the tellurium inclusions are evenly distributed.
[0050] Furthermore, the CdZnTe material is bare 241 Am energy spectrum, and the energy resolution of gamma rays with an energy of 59.5keV is less than 7%.
[0051] Optionally, the anode 1 and the cathode are made of any one of gold, indium, silver and aluminum.
[0052] In one embodiment, based on the above embodiment, the detector body is a cuboid, and the top and bottom surfaces of the cuboid are squares, and the height of the cuboid is 1 / 2 of the side length of the square.
[0053] Optionally, the diameter of the circular electrode is 1 / 10 to 1 / 5 of the side length of the square; the height of the side ring electrode 3 is at least 4 / 5 of the height of the cuboid; the distance from the inner ring of the ring electrode 4 to the center of the top surface is 1 / 8 of the side length of the square, and the distance from the outer ring of the ring electrode 4 to the center of the top surface is 1 / 4 to 3 / 10 of the side length of the square.
[0054] In one embodiment, based on the above embodiment, referring to Figures 1 to 4 The size of the detector body is 10×10×5mm 3 The diameter of the circular electrode is 1.25 mm; the height of the side ring electrode 3 is 5 mm; the ring electrode 4 is a square ring, the distance from the inner ring of the ring electrode 4 to the center of the top surface is 1.25 mm, and the distance from the outer ring of the ring electrode 4 to the center of the top surface is 3 mm.
[0055] In this embodiment, the ring electrode 4 is a square ring.
[0056] Reference Figure 1 and Figure 3 The side length of the detector body is 10mm, the diameter of the circular electrode is 1.25mm, and the distance from the inner ring of the annular electrode 4 to the center of the top surface is 1.25mm. Therefore, the shortest first distance is 0.625mm; the distance from the outer ring of the annular electrode 4 to the center of the top surface is 3mm, so the shortest second distance is 2mm.
[0057] Reference Figure 4 The height of the side ring electrode 3 and the detector body is the same as 5 mm, that is, the side ring electrode 3 completely covers the side of the detector body (including four sides, Figure 4 This is a one-side example only).
[0058] Preferably, the insulating layer 7 is made of aluminum oxide and has a resistivity of 10 14 Ω•cm; the anode 1 and cathode materials are gold.
[0059] Reference Figure 5 , Figure 5 The structure of the detector in which the annular electrode is a square ring and the structure without an annular electrode on the top surface of the detector are 137 Cs energy spectrum comparison diagram; wherein, the energy spectrum corresponding to the ring-less electrode is the first energy spectrum, and the energy spectrum corresponding to the ring electrode as a square ring is the second energy spectrum. From the comparison of the first energy spectrum and the second energy spectrum, it can be seen that the various full-energy peak characteristics of the detector structure of this embodiment are superior to the various full-energy peak characteristics of the detector structure without ring electrodes; wherein, the various full-energy peak characteristics of the two (including photoelectric peak address, full-energy peak height, peak full width (FWTM), peak-to-compton ratio (P / C)) are shown in the following Table 1:
[0060] Table 1:
[0061] Detector structure No ring electrode Ring electrode is square ring Photoelectric Peak Address 612 635 All-round peak 67698 102285 Full Width Peak (FWTM) 47 26 Peak to Compact Ratio (P / C) 2.93 4.76
[0062] It can be seen that the quasi-hemispherical CdZnTe detector structure in this embodiment increases the total energy peak count, increases the photoelectric peak address, and improves the overall charge collection efficiency of the detector. In this way, the peak shape characteristics of the energy spectrum obtained by the quasi-hemispherical CdZnTe detector structure are better, the low-energy tailing is greatly reduced, the full width of the photoelectric peak is reduced, and the peak-to-compton ratio is greatly improved.
[0063] In one embodiment, based on the above embodiment, referring to Figures 6 to 9 The size of the detector body is 10×10×5mm 3 The diameter of the circular electrode is 2 mm; the height of the side ring electrode 3 is 4 mm; the ring electrode 4 is a circular ring, the distance from the inner ring of the ring electrode 4 to the center of the top surface is 1.25 mm, and the distance from the outer ring of the ring electrode 4 to the center of the top surface is 2.5 mm.
[0064] In this embodiment, the annular electrode 4 is a circular ring.
[0065] Reference Figure 6 and Figure 8 The side length of the detector body is 10mm, the diameter of the circular electrode is 2mm, and the distance from the inner ring of the annular electrode 4 to the center of the top surface is 1.25mm, so the shortest first distance is 0.25mm; the distance from the outer ring of the annular electrode 4 to the center of the top surface is 2.5mm, so the shortest second distance is 2.5mm.
[0066] Reference Fig. 9 , the height of the side ring electrode 3 is 4 mm, and the height of the detector body is 5 mm, then the side ring electrode 3 partially covers the side of the detector body (including four side surfaces, Figure 4 This is a one-side example only).
[0067] Preferably, the insulating layer 7 is made of aluminum oxide and has a resistivity of 10 14 Ω•cm; the anode 1 and cathode materials are gold.
[0068] Reference Fig.10 , Fig.10 The structure of the detector in which the annular electrode is a circular ring and the structure without an annular electrode on the top surface of the detector are 137 Cs energy spectrum comparison diagram; wherein, the energy spectrum corresponding to the ringless electrode is the first energy spectrum, and the energy spectrum corresponding to the ring electrode as a circular ring is the third energy spectrum. From the comparison of the first energy spectrum and the third energy spectrum, it can be seen that the various full-energy peak characteristics of the detector structure of this embodiment are superior to the various full-energy peak characteristics of the detector structure without a ring electrode; wherein, the various full-energy peak characteristics of the two (including photoelectric peak address, full-energy peak height, peak full width (FWTM), peak-to-compton ratio (P / C)) are shown in the following Table 2:
[0069] Table 2:
[0070] Detector structure No ring electrode Ring electrode is a ring Photoelectric Peak Address 613 627 All-round peak 49387 94978 Full Width Peak (FWTM) 66 28 Peak to Compact Ratio (P / C) 2.14 4.32
[0071] It can be seen that the quasi-hemispherical CdZnTe detector structure in this embodiment increases the total energy peak count, increases the photoelectric peak address, and improves the overall charge collection efficiency of the detector. In this way, the peak shape characteristics of the energy spectrum obtained by the quasi-hemispherical CdZnTe detector structure are better, the low-energy tailing is greatly reduced, the full width of the photoelectric peak is reduced, and the peak-to-compton ratio is greatly improved.
[0072] In summary, a quasi-hemispherical CdZnTe detector with improved full-energy peak shape characteristics provided in the embodiments of the present application ensures that the weight potential of the anode pixels of the quasi-hemispherical detector is optimized, while ensuring the effect of optimizing the weight potential of small pixels, increasing the electric field strength in most areas within the detector volume, and effectively improving the charge collection efficiency of the quasi-hemispherical CdZnTe detector, thereby improving the full-energy peak shape characteristics, including increasing the full-energy peak height, increasing the peak-to-Compton ratio, and reducing the full width of the peak (FWTM).
[0073] It should be noted that, in this article, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, device, article or method including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, device, article or method. In the absence of further restrictions, an element defined by the sentence "includes a ..." does not exclude the presence of other identical elements in the process, device, article or method including the element.
[0074] The above description is only a preferred embodiment of the present application, and does not limit the patent scope of the present application. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly used in other related technical fields, are also included in the patent protection scope of the present application.
Claims
1. A quasi-hemispherical CdZnTe detector that improves the peak shape of the full energy peak. It is characterized in that include: The detector body, the anode and the cathode; wherein the anode is a circular electrode arranged on the top surface of the detector body, and the center of the circle is located at the center of the top surface; the cathode includes a plane electrode covering the bottom surface of the detector body, a side ring electrode wrapping the side surface of the detector body, and a ring electrode surrounding the anode; There is a first distance between the inner ring of the annular electrode and the anode, a second distance between the outer ring of the annular electrode and the side edge of the top surface of the detector body, and an insulating layer is provided between the annular electrode and the top surface of the detector body; the positive bias voltage applied by the anode is higher than the positive bias voltage applied by the annular electrode; The side ring electrode is connected to the plane electrode and is grounded to the plane electrode; The detector body is a cuboid, and the top and bottom surfaces of the cuboid are squares, and the height of the cuboid is 1 / 2 of the side length of the square; The diameter of the circular electrode is 1 / 10 to 1 / 5 of the side length of the square; the height of the side ring electrode is at least 4 / 5 of the height of the cuboid; the distance from the inner ring of the ring electrode to the center of the top surface is 1 / 8 of the side length of the square, and the distance from the outer ring of the ring electrode to the center of the top surface is 1 / 4 to 3 / 10 of the side length of the square; the second spacing is at least 1 / 5 of the side length of the square.
2. The quasi-hemispherical CdZnTe detector according to claim 1, It is characterized in that The resistivity of the insulating layer is 10 14 Ω•cm and above.
3. The quasi-hemispherical CdZnTe detector according to claim 1, It is characterized in that The resistivity of the CdZnTe material used in the detector body is 10 9 Ω•cm or above, and the working leakage current is less than 10nA.
4. The quasi-hemispherical CdZnTe detector according to claim 3, It is characterized in that The CdZnTe material bare test 241 Am energy spectrum, and the energy resolution of gamma rays with an energy of 59.5keV is less than 7%.
5. The quasi-hemispherical CdZnTe detector according to claim 1, It is characterized in that The positive bias voltage applied to the anode is 1000V, and the positive bias voltage applied to the ring electrode is 500V.
6. The quasi-hemispherical CdZnTe detector according to claim 1, It is characterized in that The material of the anode and the cathode is any one of gold, indium, silver and aluminum.
7. The quasi-hemispherical CdZnTe detector according to claim 1, It is characterized in that The size of the detector body is 10×10×5 mm 3 The diameter of the circular electrode is 1.25 mm; the height of the side ring electrode is 5 mm; the ring electrode is a square ring, the distance from the inner ring of the ring electrode to the center of the top surface is 1.25 mm, and the distance from the outer ring of the ring electrode to the center of the top surface is 3 mm.
8. The quasi-hemispherical CdZnTe detector according to claim 1, It is characterized in that The size of the detector body is 10×10×5 mm 3 The diameter of the circular electrode is 2 mm; the height of the side ring electrode is 4 mm; the ring electrode is a circular ring, the distance from the inner ring of the ring electrode to the center of the top surface is 1.25 mm, and the distance from the outer ring of the ring electrode to the center of the top surface is 2.5 mm.
Citation Information
Patent Citations
Coplanar gate anode tellurium-zinc-cadmium detector with capacitor gate and method for making same
CN101038942A
Semiconductor detector
CN103235332A
Hemispherical tellurium-zinc-cadmium detector and three-dimensional position reconstruction method
CN118011456A
Semiconductor radiation detector with enhanced charge collection
CN1203669A
Radiation detector and radiation apparatus
US20050098730A1