A modified sepiolite adsorbent and its preparation method and application
Through the preparation of modified sepiolite adsorbent, its strong affinity is used to improve the adsorption effect of benzene series, which solves the problem of poor benzene series removal effect in the existing technology and achieves efficient and low-cost sewage treatment. and supports reuse of adsorbents.
Patent Information
- Application Number
- CN202411078589.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-08-07
AI Technical Summary
When the existing technology treats benzene-containing organic sewage, the removal effect of the adsorbent is not ideal, especially benzene compounds that are highly toxic to organisms, affecting sludge activity and treatment efficiency.
Using the preparation method of modified sepiolite adsorbent, through the grafting reaction of sepiolite and epichlorohydrin and coating with bisphenol A type epoxy resin, bisphenol A type epoxy resin modified sepiolite adsorption is formed agent, using its strong affinity to improve the adsorption capacity of benzene series.
It achieves the removal effect of more than 99% of benzene series such as p-chlorobenzene, phenol, dichlorophenol, nitrobenzene, xylene, etc. It is easy to operate, low cost, and the adsorbent can be reused without generating solid waste.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the field of wastewater / sewage treatment, and in particular relates to a modified sepiolite adsorbent and a preparation method and application thereof. Background Art
[0002] The extensive use of organic pesticides and hormone drugs has caused an increase in the content of benzene-based organic pollutants in the water environment. Since these substances have high biological toxicity and a long metabolic cycle in the natural environment, they have caused great harm to organisms and humans. Therefore, it is of great significance to develop efficient and low-cost sewage treatment technology for these pollutants.
[0003] At present, the main methods for treating wastewater containing benzene series are physical, chemical and biological methods. The physical method refers to the use of basic physical theories to remove water pollutants through adsorption, precipitation, flocculation and other processes. The chemical method refers to the use of oxidation-reduction methods to decompose organic matter in water into harmless substances. The biological method refers to the use of microorganisms to digest and absorb organic matter as a component of the organism, or convert it into non-toxic inorganic and organic small molecules. The biological method is simple to operate and easy to use on a large scale, but some benzene series are biologically toxic, which affects the activity of sludge and causes low treatment efficiency. Coagulation, sedimentation and adsorption methods are to transfer organic matter from liquid to solid surface, but the current adsorbent removal effect still needs to be improved. Summary of the invention
[0004] The technical problem to be solved by the present invention is to overcome the deficiencies and defects mentioned in the above background technology and provide a modified sepiolite adsorbent and a preparation method and application thereof to improve the removal effect of benzene-containing organic pollutants.
[0005] In order to solve the above technical problems, the technical solution proposed by the present invention is:
[0006] A method for preparing a modified sepiolite adsorbent comprises the following steps:
[0007] S1. The substrate is grafted with epichlorohydrin to generate a sepiolite having an epoxy group grafted thereon; the substrate is sepiolite or alkali-modified sepiolite; the grafting reaction comprises an organic solvent as a reaction solvent, an alkaline ionic liquid as a catalyst, and an inorganic base as a cyclizing agent;
[0008] S2. The epoxy group-grafted sepiolite obtained in step S1, bisphenol A, epichlorohydrin and an inorganic strong base are subjected to a polymerization reaction in a solvent to obtain a bisphenol A type epoxy resin modified sepiolite adsorbent.
[0009] As a further improvement, the product after the grafting reaction in step S1 is extracted with methanol and dried to achieve product purification; the product after the polymerization reaction in step S2 is washed and dried to obtain a bisphenol A type epoxy resin modified sepiolite adsorbent.
[0010] As a further improvement, the amount of epichlorohydrin used in step S1 is 2-10% of the mass of the substrate.
[0011] As a further improvement, the alkaline ionic liquid in step S1 includes one or more of 1-ethyl-3-methylimidazolium dicyanomethylene, tetrabutylammonium hydroxide, or 1-ethyl-3-methylimidazolium acetate. The amount of the alkaline ionic liquid is 1-5% of the mass of epichlorohydrin.
[0012] As a further improvement, the inorganic strong base is a sodium hydroxide or potassium hydroxide solution, and the mass ratio of the sodium hydroxide or potassium hydroxide contained in the solution to the epichlorohydrin is (1~2):1.
[0013] As a further improvement, the amount of bisphenol A used in step S2 is 5-20% of the mass of the epoxy group-grafted sepiolite.
[0014] As a further improvement, the amount of epichlorohydrin used in step S2 is twice the amount of bisphenol A used.
[0015] As a further improvement, the grafting reaction temperature in step S1 is 70-110°C, and the polymerization reaction temperature in step S2 is 70-110°C.
[0016] The invention also provides a modified sepiolite adsorbent prepared by the preparation method.
[0017] The present invention also provides an application of the modified sepiolite adsorbent in treating organic wastewater containing benzene series.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The present invention utilizes sepiolite as a base material and adopts a bisphenol A epoxy resin coating method to modify the sepiolite to prepare a bisphenol A epoxy resin modified sepiolite adsorbent. The present invention not only utilizes the adsorption and hydrophilicity of sepiolite to organic matter, but also utilizes the strong affinity of bisphenol A epoxy resin to benzene series to improve the wastewater treatment rate, thereby enhancing the adsorption capacity of sepiolite for treating wastewater containing benzene series organic pollutants.
[0020] The bisphenol A epoxy resin modified sepiolite adsorbent prepared by the present invention is used to treat organic wastewater. When the benzene-containing organic pollutants in the organic wastewater are chlorobenzene, phenol, dichlorophenol, nitrobenzene and xylene, the adsorbent can achieve a removal effect of up to 99%.
[0021] The adsorbent prepared by the method of the present invention is easy to operate and low in cost when used. After the treatment is completed, the adsorbent can be further recycled and no solid waste is generated. DETAILED DESCRIPTION
[0022] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and carefully in combination with preferred embodiments below, but the protection scope of the present invention is not limited to the following specific embodiments.
[0023] Unless otherwise defined, all professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0024] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.
[0025] The adsorbent of the present invention is based on natural sepiolite or alkali-modified sepiolite after drying, and its preparation method comprises:
[0026] S1. The substrate is grafted with epichlorohydrin to form a sepiolite having epoxy groups grafted thereon.
[0027] In some embodiments, the substrate can be natural fibrous sepiolite or sepiolite modified by alkali such as sodium hydroxide or potassium hydroxide, and the particle size of the sepiolite is 20-300 meshes. It is vacuum dried before use, and the vacuum drying temperature can be 80-120° C., and the vacuum drying time is 4-8 hours.
[0028] In some embodiments, the grafting reaction uses an organic solvent as a reaction solvent, an alkaline ionic liquid as a catalyst, and an inorganic strong base as a cyclizing agent, and under certain conditions, the above substances undergo etherification and cyclization reactions to prepare sepiolite grafted with epoxy groups.
[0029] In some embodiments, the amount of epichlorohydrin used is 2-10% of the mass of sepiolite.
[0030] In some embodiments, the organic solvent may be an aprotic solvent such as acetone, tetrahydrofuran, chloroform, 1,4-dioxane, 1,2-chloroethane, 1,2-dichloropropane, etc. The amount of the organic solvent used is 4 to 8 times the mass of the sepiolite.
[0031] In some embodiments, the alkaline ionic liquid catalyst includes one or more of 1-ethyl-3-methylimidazolium dicyanomethylene, tetrabutylammonium hydroxide, and 1-ethyl-3-methylimidazolium acetate. The amount of the catalyst is 1-5% of the mass of epichlorohydrin. In the grafting reaction, the alkaline ionic liquid is necessary. Without the addition of the alkaline ionic liquid, the grafting of the epoxy group cannot be achieved.
[0032] In some embodiments, the inorganic strong base is sodium hydroxide or potassium hydroxide solution, the solution concentration is 20-50% (wt), and the mass ratio of sodium hydroxide to epichlorohydrin contained in the solution is (1-2):1.
[0033] In some embodiments, the grafting reaction temperature is 70-110° C., and the reaction time is 4-8 hours.
[0034] In some embodiments, after the grafting reaction is completed, the product is extracted with methanol to remove organic matter and solvent that have not participated in the reaction, and then dried to purify the product.
[0035] S2. The epoxy group-grafted sepiolite obtained in step S1, bisphenol A, epichlorohydrin, and an inorganic strong base are polymerized in a solvent in a certain proportion, and the sepiolite is modified by coating the bisphenol A epoxy resin generated by the reaction, and then washed and dried to obtain a bisphenol A epoxy resin-modified sepiolite adsorbent.
[0036] In some embodiments, the amount of bisphenol A used is 5-20% of the mass of the grafted sepiolite. The amount of epichlorohydrin used is twice the amount of bisphenol A used.
[0037] In some embodiments, the inorganic strong base is sodium hydroxide or potassium hydroxide solution, the solution concentration is 20-50% (wt), and the mass ratio of sodium hydroxide to epichlorohydrin contained in the solution is (1-2):1.
[0038] In some embodiments, the solvent used in the polymerization reaction can be acetone, tetrahydrofuran, chloroform, 1,4-dioxane, 1,2-ethyl chloride, and the amount used is 4 to 8 times the mass of the grafted sepiolite.
[0039] In some embodiments, the polymerization reaction temperature is 70-110° C., and the reaction time is 4-8 h.
[0040] In some embodiments, the washing solvent may be ethyl acetate or chloroform. The drying temperature is 80-120° C. and the drying time is 4-8 hours.
[0041] Both bisphenol A and epoxy groups are electronegative, and this type of structure contains more delocalized electrons and π electron structures. At the same time, there are also more delocalized electrons and π electrons on benzene derivatives, which will form a strong π electron interaction between them, thus facilitating the adsorption and removal of benzene derivatives.
[0042] By changing the ratio of epichlorohydrin to sepiolite, grafted sepiolite with different numbers of epoxy groups can be obtained, and by changing the ratio of bisphenol A, epichlorohydrin, and grafted sepiolite, bisphenol A-type epoxy resin modified sepiolite adsorbent with different bisphenol A group contents can be obtained. The content of epoxy groups and bisphenol A groups determines the adsorption capacity of the adsorbent for organic pollutants containing benzene in water bodies. At the same time, the introduction of organic matter can also change the hydrophobicity of sepiolite, and the change in hydrophobicity can also adjust the adsorption capacity of the adsorbent for benzene series or organic matter containing benzene.
[0043] The present invention evaluates the performance of the adsorbent by removing the organic matter in the simulated wastewater containing benzene series. The benzene series can be chlorobenzene, phenol, dichlorophenol, nitrobenzene, xylene and the like.
[0044] The bisphenol A epoxy resin modified sepiolite adsorbent of the present invention can be regenerated by an organic solvent to achieve repeated use. For example, the modified sepiolite adsorbent after treating wastewater is soaked in methanol for 10 to 15 hours, and then filtered and dried.
[0045] Example 1
[0046] S1. Pre-treat 100 g of fibrous sepiolite in a vacuum drying oven at 100°C for 8 h for later use. Then take 500 g of 1,2-dichloropropane in a flask, add 5 g of epichlorohydrin and 0.05 g of tetrabutylammonium hydroxide, and a 20% (wt) alkaline solution containing 10 g of sodium hydroxide in the flask in sequence, and stir to fully dissolve it into a homogeneous solution. Then introduce the treated sepiolite into the flask and stir to disperse it. Stir the dispersed system at 100°C for 6 h. After the reaction is completed, cool it to room temperature, filter it with a Buchner funnel to obtain the grafted sepiolite, and then use methanol as a solvent to perform Soxhlet extraction on the crude product for 12 h (to remove organic matter and solvent that do not participate in the reaction), and then vacuum dry it at 100°C for 6 h to purify the grafted sepiolite.
[0047] S2. Take 100 grams of refined grafted sepiolite, 10 grams of bisphenol A, 20 grams of epichlorohydrin, 20% (wt) alkaline solution containing 40 grams of sodium hydroxide, and 500 grams of acetone and add them to a reaction container. Stir and react at 80°C for 6 hours. After the reaction is completed, cool to room temperature, filter with a Buchner funnel and wash with ethyl acetate. After washing, vacuum dry at 100°C for 6 hours to obtain a bisphenol A epoxy resin modified sepiolite adsorbent.
[0048] In order to explore the effect of the content of epoxy group and bisphenol A group on the performance of the adsorbent, the following examples and comparative examples were carried out on the basis of Example 1. The differences from Example 1 are listed in Table 1.
[0049] Table 1
[0050]
[0051] In which, step S1 is omitted in comparative example 2, and sepiolite is directly used as raw material in step S2. Step S2 is omitted in comparative example 4. Unmodified sepiolite is used in comparative example 5.
[0052] Performance evaluation: Take 1 gram of the adsorbent material prepared in the above Examples 1-5 and Comparative Examples 1-5, respectively, add them to 1 liter of 100 mg / L dichlorophenol solution, stir and adsorb for 30 minutes, and after the adsorption is completed, take the supernatant with a syringe filter, and test the change in the concentration of dichlorophenol before and after adsorption by ultraviolet spectrophotometry, and calculate the removal rate of dichlorophenol: dichlorophenol removal rate = (1-concentration of dichlorophenol after adsorption / concentration of dichlorophenol before adsorption) × 100%.
[0053] According to the test results, the changes in the concentrations of the solutions before and after the adsorption treatment by the adsorbent materials prepared in Examples 1-5 and Comparative Examples 1-5 and the removal rates of dichlorophenol are shown in Table 2.
[0054] Table 2
[0055]
[0056] The adsorbed material is placed in a methanol solution with a mass of 10 times that of the original material and soaked for 12 hours, then filtered and dried to achieve regeneration and reuse.
[0057] The bisphenol A epoxy resin modified sepiolite adsorbents of Examples 1-5 after the above adsorption were respectively placed in 10 grams of methanol solution and soaked for 12 hours, then filtered and vacuum dried at 80°C for 4 hours, and then added to 1 liter of 100 mg / L dichlorophenol solution and stirred for adsorption for 30 minutes. After the adsorption was completed, the supernatant was taken with a needle filter, and the concentration change of dichlorophenol before and after adsorption was tested by ultraviolet spectrophotometry, and the removal rate of dichlorophenol was calculated. The specific results are shown in Table 3.
[0058] Table 3
[0059]
[0060] The data results show that the bisphenol A epoxy resin modified sepiolite adsorbent of the present invention can be regenerated by methanol solution and reused.
[0061] The above is only a preferred embodiment of the present invention and does not limit the present invention in any form. Therefore, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the content of the technical solution of the present invention shall fall within the scope of protection of the technical solution of the present invention.
Claims
1. A method for preparing a modified sepiolite adsorbent, characterized in that: The steps include: S1. The substrate is grafted with epichlorohydrin to form a sepiolite grafted with epoxy groups; the substrate is sepiolite or alkali-modified sepiolite; the grafting reaction uses an organic solvent as a reaction solvent, an alkaline ionic liquid as a catalyst, and an inorganic strong base as a cyclizing agent; the amount of epichlorohydrin used is 2 to 10% of the mass of the substrate; S2. The epoxy group-grafted sepiolite obtained in step S1, bisphenol A, epichlorohydrin and an inorganic strong base are polymerized in a solvent to obtain a bisphenol A-type epoxy resin modified sepiolite adsorbent; the amount of bisphenol A is 5 to 20% of the mass of the epoxy group-grafted sepiolite.
2. The method for preparing the modified sepiolite adsorbent according to claim 1, characterized in that: The product after the grafting reaction in step S1 is extracted with methanol and dried to achieve product purification; the product after the polymerization reaction in step S2 is washed and dried to obtain a bisphenol A type epoxy resin modified sepiolite adsorbent.
3. The method for preparing the modified sepiolite adsorbent according to claim 1, characterized in that: The alkaline ionic liquid in step S1 includes one or more of 1-ethyl-3-methylimidazolium dicyanomethylene, tetrabutylammonium hydroxide, or 1-ethyl-3-methylimidazolium acetate, and the amount of the alkaline ionic liquid is 1-5% of the mass of epichlorohydrin.
4. The method for preparing the modified sepiolite adsorbent according to claim 1 or 2, characterized in that: The inorganic strong base in steps S1 and S2 is a sodium hydroxide solution or a potassium hydroxide solution, and the mass ratio of the sodium hydroxide or potassium hydroxide contained in the solution to the epichlorohydrin is (1-2):
1.
5. The method for preparing the modified sepiolite adsorbent according to claim 1 or 2, characterized in that: The amount of epichlorohydrin used in step S2 is twice the amount of bisphenol A used.
6. The method for preparing the modified sepiolite adsorbent according to claim 1 or 2, characterized in that: The grafting reaction temperature in step S1 is 70-110°C, and the polymerization reaction temperature in step S2 is 70-110°C.
7. A modified sepiolite adsorbent prepared by the preparation method according to any one of claims 1 to 6.
8. Use of the modified sepiolite adsorbent according to claim 7 in treating organic wastewater containing benzene series.